Longitudinal Joint Experience Jay Behnke, P.E. Owner/President S.T.A.T.E. Testing, LLC 2017 Illinois Bituminous Paving Conference December 12, 2017

Upload: others

Post on 21-May-2020

8 views

Category:

Documents


0 download

TRANSCRIPT

Page 1: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Longitudinal Joint Experience

Jay Behnke, P.E.Owner/President S.T.A.T.E. Testing, LLC

2017 Illinois Bituminous Paving ConferenceDecember 12, 2017

Page 2: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

2

Our Sand Box

Illinois

Wisconsin

Presenter
Presentation Notes
Who we are: Chicago, O’Hare several large counties IL Tollway
Page 3: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Industry Accomplishments

Rutting• Moving from Marshall to Superpave, Volumetrics

Tackling segregation• MTD, lower Va, smaller NMAS

Stripping• T283, Hamburg

Cracking• DCT, IFIT, Recovered PG Grading

Page 4: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Longitudinal Joints

WEAK LINK

Page 5: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Weak Link….

Presenter
Presentation Notes
Any of us that drive our highways can’t help but notice poor joint performance
Page 6: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Water Intrusion Into Pavement

Presenter
Presentation Notes
May be a little hard to see, but joint has water ponding in joint. Joints allow water intrusion into pavement where freeze thaw action damages pavement. If we can keep water out, overall pavement performs better.
Page 7: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Maintenance Expensive and Disruptive

Presenter
Presentation Notes
Better to improve during initial construction
Page 8: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

How do we fix this issue?

Preventing Longitudinal Joint failure is MUCH cheaper than maintaining a joint throughout the life of the pavement

Page 9: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Many agencies are getting involved

Page 10: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

WHRP Longitudinal Joint Study

•Researched in-place data for:

•Joint Type (vertical, notched wedged etc.)

•Joint Method (rolling on, overhang or back from joint)

Page 11: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Longitudinal Joint Type

• Echelon

• Notched Wedge

• Normal Vertical

• Safety Edge

• Milled

Lane 1 Lane 2

Page 12: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

WisDOT Joint Data

•1400 data sets•28 projects•No joint density > 93%

Page 13: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

WHRP Study Recommendations

•Joint Type:• Notched Wedge / Mill out wedge

•Joint Method:• Unconfined: Stay back from edge with Roller

(WI uses fine graded mixes)

• Confined: Type of rolling pattern did not make a difference

Page 14: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

WHRP Study Recommendations

Page 15: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Make it better??

Page 16: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

IDOT District 4 Mill Wide Pave Wide Experiment Approach

Presenter
Presentation Notes
D-4 trials with milling 6 inches wide to remove unconfined low density material. Produced much improved density results. However, If for no other reason, traffic control in urban areas would be a problem.
Page 17: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

D-4 Pave Wide Mill Wide

Page 18: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Concerns:

1. Urban Areas• Time factor• Perception

2. Permeability• Isn’t fully addressed

Page 19: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Agree to DisagreeHey – Teddy Brosevelt!

Why not LJS?

Mill off unconfined

joint?

Page 20: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Need to prevent Permeability

•Increase density (obviously)•Brother from a Different Mother:• Longitudinal Joint Seal (LJS) –

IDOT• Void Reducing Asphalt Material

(VRAM) - Tollway• J-Band = Joint Band – Heritage

proprietary

Page 21: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

IDOT Policy and Spec March 2017

Presenter
Presentation Notes
Credit to IDOT CBM for long term emphasize and research
Page 22: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Suppliers (3 on IDOT list)

Presenter
Presentation Notes
Credit to IDOT CBM for long term emphasize and research
Page 23: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Application Rates:

Page 24: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Bid Tabs on I-55 in 2016

Please Note: • These are large quantities • LJS is at 12” (for SMA) & 15% less• LJS should be 18” for dense graded

Page 25: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Long Term Experience 14 Years Later

Route 26 Conventional Joint

Route 26 with Joint Sealant

Presenter
Presentation Notes
14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant (Quickseam), which would meet LGS is in great shape.
Page 26: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

No Maintenance After 14 Years

Route 50 Conventional Route 50 J-Band

Presenter
Presentation Notes
14 years old. Conventional section has required maintenance. J-band section has required none. Illinois Route 50 in D-1. Thanks to IDOT for the slides
Page 27: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Distributors Improving

Page 28: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

DuPage County

•Wanted improved longitudinal joint performance

•Started specifying alternative methods in 2013• Echelon Paving• Infra-red Joint Heater• J-Band

•Performance testing on joint cores

Page 29: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Tested Right ON the Joint!

Page 30: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

DuPage County

•Joint treatment types tested:• J-Band (Bid @ $2.80 per foot)• Echelon (Incidental)• Infra-red Joint Heater (Incidental)

•4 x 150mm cores directly over the joint•Performance test results (DCT & I-FIT)

Page 31: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

DuPage County – Gary Ave.

Mix Type Vir AC Section TypeDCT

(J/m²)I-FIT (FI)

Ave Density

N70E SBS PG70-28 J-Band 675.5 41.0 98.9¹N70E SBS PG70-28 Echelon 485.5 14.7 94.1N70E SBS PG70-28 Joint Heater 418.5 12.3 90.4

2016 DuPage North - Gary Avenue

1 - Gmm calculated from cores

Results!

Page 32: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

DuPage County – Hobson Rd.

Mix Type Vir AC Section TypeDCT

(J/m²)I-FIT (FI)

Ave Density

N70E SBS PG70-28 J-Band 395.5 48.5 95.7¹N70E SBS PG70-28 Echelon 418.5 10.7 93.3N70E SBS PG70-28 Joint Heater 340.0 11.0 92.8

2016 DuPage South - Hobson Road

1 - Gmm calculated from cores

Page 33: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Conclusions DuPage County.

LJS and Echelon are the only approved methods going forward

Page 34: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

I-88 Tollway Trials

•Tollway Trials and Innovations• RAP fractionation• Warm mix mandate• RAS implementation• GTR trials and use• And a whole lot of other ones!

• LJS in 2015 Torque Test

Page 35: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Brought to you by:

Page 36: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

V-RAM

Page 37: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

I-88 Field Trials

•Migration•Hamburg•Single Edge Notch Disk•Torque Test

Page 38: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Learning Experience

•Flushing observed after application on SMA

•Application rate reduced in current IDOT specification

Page 39: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Hamburg Results

Flushed areas did not show increased rutting potential

Presenter
Presentation Notes
The results don’t pass the <6mm Hamburg SMA spec but keep in mind that these cores are taken directly adjacent to the joint and is more for a comparison”
Page 40: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

CDOT All Aboard!

Page 41: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

CDOT Arterial Resurfacing Program 2016

•Contract divided into four quadrants of City

•Each required joint treatment on one street

•Trials used IDOT Longitudinal Joint Treatment

•Two completed in 2016•Two completed in 2017

Page 42: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

LJS Constructibility

• Sets up in a few minutes

• Does not pick up under traffic. (Note tire tracks but no pickup)

Page 43: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

DCT Results – CDOT

*PG 70-28 is SBS polymerized

**

Results!

Page 44: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

DCT Results at Joint

•DCT higher for lower quality mix with a neat PG58-28 AC than mix with SBS polymer PG70-28

•Filling voids with the LJS has a greater effect on the mix properties at joint than polymer AC.

Page 45: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

CDOT Field Experience

•Experience positive

•Will be using on more projects

Page 46: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

CDOT Implementation 2017

•City-wide Term Contracts (3 year term, 4 set areas, mixes, etc.) included LJS

•79,000 LF for the quantity per contract area•Bigane Paving low bidder on all four contracts•Unit price was $3.00 to $3.50 /LF on each contract

Page 47: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

CDOT Arterial 2017

•Bid opening was late fall 2017• North 183,285ft; $2.00/ft• Central 161,780ft; $2.00/ft• South 140,178ft; $2.00/ft• Far South 201,172ft; $1.95/ft

•Started paving this year (Cold temps/No Issues)•Will finish balance in 2018•ALL locations get LJS!!

Page 48: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Conclusion

•Variety of approaches to improve performance at joint – most don’t work

•My recommendation is ….

LJS

Page 49: Longitudinal Joint Experience - Illinois · Longitudinal Joint Experience Jay Behnke, P.E. ... 14 year old job. Illinois 26 in D-2. Conventional joint distressed. Joint using a sealant

Questions?