From dilute to condensed magnetic semiconductors:a protocol for systematic characterization
Mauro Rovezzi1
1Institute for Semiconductors and Solid State Physics, Johannes Kepler University, Linz, Austria
[W. Stefanowicz et al., arXiv.org 0912.4216 (2010)][A. Navarro-Quezada et al., Phys. Rev. B 81, 205206 (2010)]
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 1 / 32
![Page 2: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/2.jpg)
Co-authors
A. Navarro-Quezada, B. Faina, T. Devillers, T. Li, A. rois, T. Winkler,A. BonanniInstitute for Semiconductors and Solid State Physics, Johannes KeplerUniversity, Linz, Austria
W. Stefanowicz, D. Sztenkiel, R. Jakiela, M. Sawicki, T. DietlInstitute of Physics, Polish Academy of Sciences, Warsaw, Poland
R. T. Lechner, G. BauerInstitute for Semiconductors and Solid State Physics, Johannes KeplerUniversity, Linz, Austria
F. d’AcapitoItalian National Research Council, IOM-OGG, c/o ESRF GILDA,Grenoble, France
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 2 / 32
![Page 3: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/3.jpg)
Outline
1 Introduction
2 Growth characterization protocol
3 Case studiesDilute (Ga,Mn)NFe segregation in GaN
4 Conclusions
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 3 / 32
![Page 4: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/4.jpg)
IntroductionBuilding-blocks for Spintronics devices
[A. Bonanni and T. Dietl, Chem. Soc. Rev. (2010)]M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 4 / 32
![Page 5: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/5.jpg)
DMS→ (Ga,Mn)N
With holes→ sp-d Zener model
x=5% and 3.5×1020 h/cm3
[T. Dietl et al., Science (2000)]
Without holes→ double exchange
[K. Sato et al., Phys. Rev. B (2004)]
[L. Berqvist et al., Phys. Rev. Lett. (2004)]
Controversial experimental reports⇒ accurate nanoscale characterization
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 5 / 32
![Page 6: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/6.jpg)
DMS→ (Ga,Mn)N
With holes→ sp-d Zener model
x=5% and 3.5×1020 h/cm3
[T. Dietl et al., Science (2000)]
Without holes→ double exchange
[K. Sato et al., Phys. Rev. B (2004)]
[L. Berqvist et al., Phys. Rev. Lett. (2004)]
Controversial experimental reports⇒ accurate nanoscale characterization
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 5 / 32
![Page 7: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/7.jpg)
DMS→ (Ga,Mn)N
With holes→ sp-d Zener model
x=5% and 3.5×1020 h/cm3
[T. Dietl et al., Science (2000)]
Without holes→ double exchange
[K. Sato et al., Phys. Rev. B (2004)]
[L. Berqvist et al., Phys. Rev. Lett. (2004)]
Controversial experimental reports⇒ accurate nanoscale characterization
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 5 / 32
![Page 8: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/8.jpg)
CMS→ (Ga,Fe)N
TMs solubility in (most) semiconductors at thermal equilibrium is low⇒ chemical/crystallographic phase separation⇒ a priori unknown magnetic properties⇒ mostly high TC FM
Examples of chemical phase separation (spinodal decomposition in DMS literature)
(Ga,Mn)As annealing
[M. Moreno et al., J. Appl.Phys. (2002)]
(Ga,Mn)N clusters
[G. Martinez-Criado et al., Appl.Phys. Lett. (2005)]
(Ge,Mn) nano-columns
[M. Jamet et al., Nature Mat.(2006)]
Detection and control of phase separation⇒ nano-characterization tools
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 6 / 32
![Page 9: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/9.jpg)
CMS→ (Ga,Fe)N
TMs solubility in (most) semiconductors at thermal equilibrium is low⇒ chemical/crystallographic phase separation⇒ a priori unknown magnetic properties⇒ mostly high TC FM
Examples of chemical phase separation (spinodal decomposition in DMS literature)
(Ga,Mn)As annealing
[M. Moreno et al., J. Appl.Phys. (2002)]
(Ga,Mn)N clusters
[G. Martinez-Criado et al., Appl.Phys. Lett. (2005)]
(Ge,Mn) nano-columns
[M. Jamet et al., Nature Mat.(2006)]
Detection and control of phase separation⇒ nano-characterization tools
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 6 / 32
![Page 10: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/10.jpg)
CMS→ (Ga,Fe)N
TMs solubility in (most) semiconductors at thermal equilibrium is low⇒ chemical/crystallographic phase separation⇒ a priori unknown magnetic properties⇒ mostly high TC FM
Examples of chemical phase separation (spinodal decomposition in DMS literature)
(Ga,Mn)As annealing
[M. Moreno et al., J. Appl.Phys. (2002)]
(Ga,Mn)N clusters
[G. Martinez-Criado et al., Appl.Phys. Lett. (2005)]
(Ge,Mn) nano-columns
[M. Jamet et al., Nature Mat.(2006)]
Detection and control of phase separation⇒ nano-characterization tools
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 6 / 32
![Page 11: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/11.jpg)
CMS→ (Ga,Fe)N
TMs solubility in (most) semiconductors at thermal equilibrium is low⇒ chemical/crystallographic phase separation⇒ a priori unknown magnetic properties⇒ mostly high TC FM
Examples of chemical phase separation (spinodal decomposition in DMS literature)
(Ga,Mn)As annealing
[M. Moreno et al., J. Appl.Phys. (2002)]
(Ga,Mn)N clusters
[G. Martinez-Criado et al., Appl.Phys. Lett. (2005)]
(Ge,Mn) nano-columns
[M. Jamet et al., Nature Mat.(2006)]
Detection and control of phase separation⇒ nano-characterization tools
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 6 / 32
![Page 12: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/12.jpg)
CMS→ (Ga,Fe)N
TMs solubility in (most) semiconductors at thermal equilibrium is low⇒ chemical/crystallographic phase separation⇒ a priori unknown magnetic properties⇒ mostly high TC FM
Examples of chemical phase separation (spinodal decomposition in DMS literature)
(Ga,Mn)As annealing
[M. Moreno et al., J. Appl.Phys. (2002)]
(Ga,Mn)N clusters
[G. Martinez-Criado et al., Appl.Phys. Lett. (2005)]
(Ge,Mn) nano-columns
[M. Jamet et al., Nature Mat.(2006)]
Detection and control of phase separation⇒ nano-characterization tools
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 6 / 32
![Page 13: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/13.jpg)
Growth characterization protocol
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 7 / 32
![Page 14: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/14.jpg)
Metalorganic Vapour Phase Epitaxy(Ga,Mn)N and (Ga,Fe)N[:Si]
AIXTRON 200RF horizontal reactorc-plane sapphire substratesPrecursors: TMGa, NH3, Cp2Fe, Cp2Mn, SiH4
Monitoring: ellipsometry
Well established growth procedure
1 Substrate nitridation2 LT (540 ◦C) GaN nucl. layer3 Annealing/recrystallization4 1 µm HT (1050 ◦C) GaN5 0.5 – 1 µm GaN:(Fe/Mn)[:Si]
800 – 950 ◦C50 – 490 sccm (→ 0.05 – 1 %)
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 8 / 32
![Page 15: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/15.jpg)
Limits of conventional high-resolution XRD
No evidence of second phases GaN(0002) peak broadening
⇒ Synchrotron radiation
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 9 / 32
![Page 16: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/16.jpg)
Limits of conventional high-resolution XRD
No evidence of second phases GaN(0002) peak broadening
⇒ Synchrotron radiation
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 9 / 32
![Page 17: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/17.jpg)
European Synchrotron Radiation Facility, Grenoble
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 10 / 32
![Page 18: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/18.jpg)
Case studies
1 Dilute (Ga,Mn)N [W. Stefanowicz et al., arXiv.org 0912.4216 (2010)]
2 Fe segregation in GaN
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 11 / 32
![Page 19: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/19.jpg)
TEM
Wide range of Mn concentration up to ≈ 1 at. %
Low-resolution High-resolution
Energy dispersive X-rayspectroscopy
No evidence of crystallographic phase separationNo Mn-induced defects
Is Mn really dilute? → SXRD
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 12 / 32
![Page 20: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/20.jpg)
TEM
Wide range of Mn concentration up to ≈ 1 at. %
Low-resolution High-resolution
Energy dispersive X-rayspectroscopy
No evidence of crystallographic phase separationNo Mn-induced defects
Is Mn really dilute? → SXRD
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 12 / 32
![Page 21: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/21.jpg)
SXRDMeasurements conducted on BM20 at 10 KeV
High crystal quality [from the FWHMof rocking curves around GaN(0002)]
No evidence for second phasesIncrement of the latticeparameters with Mn concentrationIn situ annealing (under N-richatmosphere) experiments→samples stable up to 900 ◦C
Where is Mn? → EXAFS
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 13 / 32
![Page 22: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/22.jpg)
SXRDMeasurements conducted on BM20 at 10 KeV
High crystal quality [from the FWHMof rocking curves around GaN(0002)]
No evidence for second phasesIncrement of the latticeparameters with Mn concentrationIn situ annealing (under N-richatmosphere) experiments→samples stable up to 900 ◦C
Where is Mn? → EXAFS
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 13 / 32
![Page 23: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/23.jpg)
EXAFSMeasurements conducted on BM08 at Mn K-edge
1 2 3 4 5 6 7 8
Mag
nitu
de o
f the
FT
, |χ(R
)| [Å
−3]
Distance, R [Å] − without phase correction
Rmin
Rmax
Mn I
TM
n IO Mn 3
GaN(b)
2 4 6 8 10 12
EX
AF
S s
igna
l, k2χ(k
)
Photoelectron wavevector, k [Å−1]
kmin kmax(a)
#490A Fit(MnGa) #100A
1 2 3 4 5 6
(c)
MnGaMn3GaN
MnIO
MnIT
Mn substitutional in GaN at Ga sites(MnGa)Low local disorderMn-Ga first shell expansion∆R=2.5(5)%Additional contributions can be ruledout in the 5% limitMn interstitial defects and Mn3GaNsimulated via ab initio codes[VASP+FEFF8]
What Mn charge state? → XANES
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 14 / 32
![Page 24: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/24.jpg)
EXAFSMeasurements conducted on BM08 at Mn K-edge
1 2 3 4 5 6 7 8
Mag
nitu
de o
f the
FT
, |χ(R
)| [Å
−3]
Distance, R [Å] − without phase correction
Rmin
Rmax
Mn I
TM
n IO Mn 3
GaN(b)
2 4 6 8 10 12
EX
AF
S s
igna
l, k2χ(k
)
Photoelectron wavevector, k [Å−1]
kmin kmax(a)
#490A Fit(MnGa) #100A
1 2 3 4 5 6
(c)
MnGaMn3GaN
MnIO
MnIT
Mn substitutional in GaN at Ga sites(MnGa)Low local disorderMn-Ga first shell expansion∆R=2.5(5)%Additional contributions can be ruledout in the 5% limitMn interstitial defects and Mn3GaNsimulated via ab initio codes[VASP+FEFF8]
What Mn charge state? → XANES
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 14 / 32
![Page 25: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/25.jpg)
Charge state
Role of TMs charge state in DMSExchange interactionsCarriers and their localizationInter-atomic Coulomb interactions
Mn in GaNMn2+ → 3d5
Mn3+ → 3d4
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 15 / 32
![Page 26: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/26.jpg)
Charge state
Role of TMs charge state in DMSExchange interactionsCarriers and their localizationInter-atomic Coulomb interactions
Mn in GaNMn2+ → 3d5
Mn3+ → 3d4
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 15 / 32
![Page 27: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/27.jpg)
XANESMeasurements conducted on BM08 at Mn K-edge
6530 6540 6550 6560 6570 6580 6590 6600 6610
No
rm.
Ab
so
rptio
n C
oe
ffic
ien
t −
µ(E
)
Energy [eV]
(b) #100A#490A
Mn(3d4)
Mn(3d5)
6535 6540 6545 6550 6555 6560 6565 6570
No
rm.
µ(E
)
(a)#100A#490A
MnOMn2O3MnO2
6537 6540 6543 6546 6549
(c)
A1A2
A3A4
BkgFit
Absorption edge shifts with thecharge state⇒ Mn3+ ⇒confirmed by pre-edge peaks
Fine-structure simulated withFDMNES⇒ MnGa
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 16 / 32
![Page 28: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/28.jpg)
SQUID
Accurate subtraction of the substrate diamagnetic signal and extra m(H,T)
Magnetization(T) Magnetization(H)
⇒ Paramagnetism from non-interacting Mn3+ ionsM. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 17 / 32
![Page 29: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/29.jpg)
SQUID
Accurate subtraction of the substrate diamagnetic signal and extra m(H,T)
Magnetization(T) Magnetization(H)
⇒ Paramagnetism from non-interacting Mn3+ ionsM. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 17 / 32
![Page 30: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/30.jpg)
Summary
Dilute (Ga,Mn)N - x ≤ 1%Mn substitutional in GaNMn3+ charge stateParamagnetic
OutlookIncrease Mn concentration (in the DMS limit)Co-doping:
(Ga,Mn)N:Si → n-type → Mn2+
(Ga,Mn)N:Mg → p-type → itinerant h
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 18 / 32
![Page 31: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/31.jpg)
Summary
Dilute (Ga,Mn)N - x ≤ 1%Mn substitutional in GaNMn3+ charge stateParamagnetic
OutlookIncrease Mn concentration (in the DMS limit)Co-doping:
(Ga,Mn)N:Si → n-type → Mn2+
(Ga,Mn)N:Mg → p-type → itinerant h
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 18 / 32
![Page 32: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/32.jpg)
Case studies
1 Dilute (Ga,Mn)N
2 Fe segregation in GaN [A. Navarro-Quezada et al., Phys. Rev. B 81, 205206 (2010)]
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 19 / 32
![Page 33: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/33.jpg)
(Ga,Fe)N: a high TC magnetic semiconductor?
Paramagnetism from isolated Fe3+ Ferromagnetism persisting aboveroom temperature
What is the origin of the ferromagnetism?
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 20 / 32
![Page 34: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/34.jpg)
(Ga,Fe)N: a high TC magnetic semiconductor?
Paramagnetism from isolated Fe3+ Ferromagnetism persisting aboveroom temperature
What is the origin of the ferromagnetism?
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 20 / 32
![Page 35: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/35.jpg)
Presence of ε-Fe3N nano-crystalsBainite structure (hexagonal), ≈ 15 nm average size, TC = 575 K
⇒ Solubility limit at ≈ 0.4 % Fe in our growth conditions
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 21 / 32
![Page 36: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/36.jpg)
Presence of ε-Fe3N nano-crystalsBainite structure (hexagonal), ≈ 15 nm average size, TC = 575 K
⇒ Solubility limit at ≈ 0.4 % Fe in our growth conditions
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 21 / 32
![Page 37: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/37.jpg)
How to control Fe incorporation in GaN?
Growth rate
Co-doping
Growth temperature
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 22 / 32
![Page 38: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/38.jpg)
Control by growth rate
⇒ Solubility limit increased by increasing the growth rate (TMGa)
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 23 / 32
![Page 39: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/39.jpg)
Control by growth rate
⇒ Solubility limit increased by increasing the growth rate (TMGa)
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 23 / 32
![Page 40: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/40.jpg)
Fermi-level engineering by co-doping with SiPartial charge state reduction, Fe3+ → Fe2+, demonstrated by XANES
Fe 3d states resides in the GaN band gapCo-doping with Si→ tuning Fermi level→ Fecharge state modificationCoulomb repulsion between Fe ions hindersaggregation [T. Dietl, Nature Mat. (2006)]
Do this really hinders the aggregation?
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 24 / 32
![Page 41: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/41.jpg)
Fermi-level engineering by co-doping with SiPartial charge state reduction, Fe3+ → Fe2+, demonstrated by XANES
Fe 3d states resides in the GaN band gapCo-doping with Si→ tuning Fermi level→ Fecharge state modificationCoulomb repulsion between Fe ions hindersaggregation [T. Dietl, Nature Mat. (2006)]
Do this really hinders the aggregation?
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 24 / 32
![Page 42: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/42.jpg)
Fermi-level engineering by co-doping with SiPartial charge state reduction, Fe3+ → Fe2+, demonstrated by XANES
Fe 3d states resides in the GaN band gapCo-doping with Si→ tuning Fermi level→ Fecharge state modificationCoulomb repulsion between Fe ions hindersaggregation [T. Dietl, Nature Mat. (2006)]
Do this really hinders the aggregation?
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 24 / 32
![Page 43: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/43.jpg)
Control by co-doping
⇒ Solubility limit increased by co-doping with SiM. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 25 / 32
![Page 44: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/44.jpg)
Control by co-doping
⇒ Solubility limit increased by co-doping with SiM. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 25 / 32
![Page 45: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/45.jpg)
Growth temperatureSXRD and TEM
Additional Fe-rich phases:γ′-Fe4N, ζ-Fe2N, α-Fe, γ-FeNano-crystals size: 10-20 nm
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 26 / 32
![Page 46: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/46.jpg)
Growth temperatureXANES & EXAFS
7110 7120 7130 7140 7150 7160 7170 7180 7190
Nor
m. A
bsor
ptio
n C
oeffi
cien
t − µ
(E)
[arb
. shi
ft]
Energy [eV]
EF
800 °C
850 °C
950 °C
S691S680S690Fit 3Fit 2Fit 1
1 2 3 4 5
|χ(R
)|
Distance, R [Å] − without phase correction
Rm
in
Rm
ax
Fe−NFe−Fe
Fe−Ga
XANES: linearcombination fits oftheoretical spectra(FDMNES)⇒ identificationand concentration ofdifferent phasesEXAFS: refinement of thelocal structure
SXRD, (HR)TEM and XAS⇒ phase-diagram of FexNy in GaN
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 27 / 32
![Page 47: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/47.jpg)
Growth temperatureXANES & EXAFS
7110 7120 7130 7140 7150 7160 7170 7180 7190
Nor
m. A
bsor
ptio
n C
oeffi
cien
t − µ
(E)
[arb
. shi
ft]
Energy [eV]
EF
800 °C
850 °C
950 °C
S691S680S690Fit 3Fit 2Fit 1
1 2 3 4 5
|χ(R
)|
Distance, R [Å] − without phase correction
Rm
in
Rm
ax
Fe−NFe−Fe
Fe−Ga
XANES: linearcombination fits oftheoretical spectra(FDMNES)⇒ identificationand concentration ofdifferent phasesEXAFS: refinement of thelocal structure
SXRD, (HR)TEM and XAS⇒ phase-diagram of FexNy in GaN
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 27 / 32
![Page 48: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/48.jpg)
Growth temperatureSQUID
Paramagnetic part⇒dilute and non-interactingFeGa
Superparamagnetic-likepart⇒ ferromagneticε-Fe3N, γ′-Fe4N α-Fe andγ-FeAntiferromagneticcomponent⇒ ζ-Fe2N andhighly-nitrated FexN (x≤2)phases
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 28 / 32
![Page 49: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/49.jpg)
Summary
Segregated (Ga,Fe)NHigh TC FM→ ε-Fe3N clustersSolubility limit controlled by→ growth-rate→ co-doping
Growth temperature→ additional FexNy phases→ wide range of magnetic behaviors
OutlookControl of single-phase FexNy in/on GaN
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 29 / 32
![Page 50: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/50.jpg)
Summary
Segregated (Ga,Fe)NHigh TC FM→ ε-Fe3N clustersSolubility limit controlled by→ growth-rate→ co-doping
Growth temperature→ additional FexNy phases→ wide range of magnetic behaviors
OutlookControl of single-phase FexNy in/on GaN
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 29 / 32
![Page 51: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/51.jpg)
CMSSecond generation spintronics devices
Spin battery
Electromotive force and hugemagnetoresistance observed inmagnetic tunnel junctions withzb-MnAs clustersDemonstrated at 30 K
[N.H. Pham et al., Nature (2009)]
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 30 / 32
![Page 52: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/52.jpg)
Conclusions
Growth characterization protocolSelf-consistent loop
1 Growth/optimization2 Structural characterization3 Magnetic characterization4 Modeling/simulation
Synchrotron radiation as required tool
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 31 / 32
![Page 53: From DMS to CMS: a characterization protocol](https://reader030.vdocuments.site/reader030/viewer/2022020207/556c90d3d8b42a7a738b4d90/html5/thumbnails/53.jpg)
Thank you for your attention!
Contact/further [email protected]
References for this work
W. Stefanowicz et al.,arXiv.org 0912.4216 (2010)→ soon in Phys. Rev. BA. Navarro-Quezada et al.,Phys. Rev. B 81, 205206 (2010)M. Rovezzi et al.,Phys. Rev. B 79, 195209 (2009)A. Bonanni et al.,Phys. Rev. Lett. 101, 135502 (2008)
M. Rovezzi (HFP/JKU) DMS & CMS characterization DEMATEN 2nd workshop (June 2010) 32 / 32