Common Defects Defect Anodizing Burn Image Defect visible after Anodizing Description Bright areas on anodic coating surrounded by black or darker area. Usually no anodic film or very soft film present in the defective area. Cause Excessive current Poor movement of electrolyte across part Poor electrical contact between rack/jig and the part. Remedy Reduce current Check electrolyte concentration and ensure temperature is controlled properly Improve electrical contact area between rack/jig and the part

Upload: others

Post on 12-Mar-2022

3 views

Category:

Documents


0 download

TRANSCRIPT

CommonDefects

Defect AnodizingBurn

Image

Defectvisibleafter Anodizing

Description • Brightareasonanodiccoatingsurroundedbyblackordarkerarea.• Usuallynoanodicfilmorverysoftfilmpresentinthedefectivearea.

Cause • Excessivecurrent• Poormovementofelectrolyteacrosspart• Poorelectricalcontactbetweenrack/jigandthepart.

Remedy • Reducecurrent• Checkelectrolyteconcentrationandensuretemperatureiscontrolledproperly• Improveelectricalcontactareabetweenrack/jigandthepart

Defect ChlorideCorrosion

Image

Defectvisibleafter Anodizing

Description Pitsformedonallsurfacesofpart.Relativelydeepandusuallyblackinappearance.Thereisnoanodicfilmoverthepits.

Cause Exceededcriticallevelofchlorideof80ppmmeasuredastheCl-ioninthesulfuricacidelectrolyte,corrodesthehighlyactivealuminumduringtheanodizingprocess.

Remedy Useofdeionizedwaterinanodizingelectrolytemake-upandtop-upandensurethoroughrinsetoeliminatingthisproblem.

Defect ColorDifferences

Image

Defectvisibleafter Coloring

Description Poorvisualcolormatch,outsidetheagreedupperandlowercolorlimits.

Cause • Alloyinconsistency• Differencesintheanodizingparameter• Incorrectdyeingconditions• Lackofcontrolofelectrolyticcoloringprocess

Remedy • Makesurethebasemetalsarefromthesamebatch.• Checkanodizingelectrolyteconcentration,PH,anodizingtimeandtemperature• Checkdyeconcentration,dyetime,temperature,PHandforcontaminationwithsulphatesand

chlorides.• Inthecaseofelectrolyticcoloring,thiscanbeduetothewrongcoloringconditionorcontaminationof

thecoloringelectrolytewithsodium.Fixrackingconfigurationtoensurecoloruniformity

Defect Crazing

Image

Defectvisibleafter Sealing

Description Hairlinecracksformintheanodiccoating.

Cause • Stressproducedintheanodicoxidecoatingwhenpartsaretransferredfromrinsetanktosealingtankduetodifferencesinthermalexpansioncoefficientbetweentheanodicoxidecoatingandthebasemetal.

• Causedbyamechanicaldeformationofananodizedpartbybendingorimpact.Canbeenhancedbyhighcurrent,lowelectrolytetemp,thickanodicfilms(hardanodizingconditions).

• Anodicoxidecoatingsexposedtohighambienttemperatures(e.g.lighting)andstrongsunlightaremorelikelytodevelopcrazingthanthoseexposedinthemoretemperateclimates

Remedy • Reducethermalshock(70°Cwaterbeforeboilingsealing)• Anybendingofthepartsshouldbecarriedoutbeforeanodizing.Preheatpartstoevenoutstressin

material(130°Cfor40min).Reducecurrent(1.4-1.6A/dm2).Electrolytetemperatureshouldbearound20°C.Reduceanodicfilmthickness(<30µm)Don’theatthickfilmabove120°C

Defect EtchStaining

Image

Defectvisibleafter Etching/Coloring

Description Stainingdevelopsonthepartafteretching.Thismaynotbeimmediatelyvisibleafteretching.

Cause • Etchingsolutiondriesonpartduringtransfertorinse• Poorcleaning/rinsingafteretching.• Poorjiggingincombinationwithpoorcleaning• Wrongetchsolutioncomposition• Etchsolutiontoohot

Remedy • Improvetimefrometchingtorinse• Ensuregoodandfastcleaning/rinsingafteretching.• Properjiggingofdifficultorthickwalledprofiledparts• Checkthelevelofwettingagentintheetchingsolutionisadequate

Ensureetchsolutiontemperatureisn’ttoohigh(<60°C)

Defect GasTrapping

Image

Defectvisibleafter Anodizing/Coloring

Description Randomspotsorareasthatareuncolored,differenthueorlighterontheundersideoftherackedworkpiece.

Cause Gasorairbubblestrappedonundersideofworkpiece.Theseairorgaspocketsactasinsulatorsforanodizingprocessormaskingagentsforthecoloringprocess

Remedy Rackpartssotherearenohorizontalsurfacesorinvertedchannelsontheundersidesogascanescape.

Defect InsufficientDegreasing

Image

Defectvisibleafter Etching/Brightening

Description NonuniformDegreasing

Cause Poordegreasesolutionorpractice(e.g.temperaturetoolow),oilorgreaseisstillleftonsomeareas.Thisleadstodifferentialetching/brighteningofthesectionsurface

Remedy Renewthedegreasingsolutionorextentthetreatmenttimeorincreasethetemperature.

Defect JigMarks

Image

Defectvisibleafter Anodizing/coloring

Description Exposedareas/marksontheanodizedpart

Cause Iftheworkpiecedonothavethreadedholes,jigmarksareinevitableasthepartsmustbeclampedtobeanodized/colored

Remedy • Usethreadedrodsinexistingthreadedholes• Selectlocationofcontactareastobeinanunimportanthiddenplace

Defect Blistering/Delaminating

Image -

Defectvisibleafter Coloring

Description Blistersformontheanodiccoatingofthework-piece.Itoccursonhighzincalloys(Aluminum7000series)

Cause Duringanodizingprocess,thealloyingelement,inthiscasezinc,whenoxidizes,istoobigtojumpthroughthealuminumoxidesporouslayerandremainsattheinterfacebetweenthesubstrateandtheanodicfilmlayer.Thisnaturallyservesasstresspointandsubsequentthermalcyclingduringcoloringprocesscausestheseareastoblister.Note:Identifydelaminationbydeterminingifacoatingispresentatthespot.Aquicktestistoapplyadropofacidifiedcoppersolution(about1Nhydrochloricacidwithabout10g/lcoppersulfate)tothespot.Ifnocoatingispresent,thespotwillturnredwithinafewminutes.

Remedy Whenanodizing,extendingtherampupperiodtoallowzinctomoveawayfromtheinterfacebetweensubstrateandtheanodicaluminumoxidelayer.Thisreducestheblisteringeffect.

Defect WhiteSpots

Image

Defectvisibleafter Afterelectrolyticcoloringordyecoloring

Description Littlewhitespotsdevelopintheanodizedlayerafterelectrolyticordyecoloration.

Cause • Whitespotthatcan’tbewipedoff,andinroundshape- Likelyduetothesurfacecontaminationthatisresultofresiduethatwasnotadequatelyremovedby

anodizerthatinhibitdyefrompickingup.Anothermaybethepresenceofalkalineparticlesfloatingaroundintheairandadheringtotheanodizesurfacewhilebeingtransferredtothedyetank.

• Whitespotthatcan’tbewipedoff,andnotinroundshape–Usuallytheresultofentrappedanodizeacidintinypits,cavitiesorgroves.Pitsmaybeduetounwantediron-containinginclusionsinthemetalthatareetchedoutduringtheanodizestep.Cavitiesmaybeduetotheporosityofcastaluminum.Tinygrovesmayoccuronmachinedsurfaces.Anodizingcanopenupsurfaceornear-surfacedefects,leavingvoidsthatcanbeverydifficulttorinseclean.Asaresult,dyepickupwillbeinhibitedintheareawhereanyacidremains.Usuallytheacidoozesoutofthepitorcavitywhileinthedyetank,formingirregularshapedspots,includingcomettails.

Remedy

• Thoroughlycleantherinsetanksorimprovefume/gasextractioninalkalineetchingstage.Topreventdisturbingaircurrentsfrometchingareatocolorationarea.

• A30-to60-secondrinsein5-10percentnitricacidfollowedbyafreshwaterrinse.