synchrotron radiation photoemission … no.3/vol.15 no.3...journal of surface analysis vol.15 no.3...

4
Journal of Surface Analysis Vol.15 No.3 (2009) pp. 303-306 Yuden Teraoka et al. Synchrotron Radiation Photoemission Spectroscopy for Native Oxide Layer on V and VCrTa 303Synchrotron Radiation Photoemission Spectroscopy for Native Oxide Layer on Vanadium and VCrTa Yuden Teraoka, Akitaka Yoshigoe, James Harries Japan Atomic Energy Agency, 1-1-1 Kouto, Sayo-cho, Sayo-gun, Hyogo 679-5148, Japan [email protected] (Received : December 29, 2008; Accepted: February 10, 2009) In order to study correlation between oxide layers on hydrogen storage metals such as V(111), polycrystalline Vanadium, and VCrTa alloy and hydrogen desorption temperature, the surfaces covered by native oxides have been analyzed by photoemission spectroscopy using soft x-ray synchrotron radiation. Depth analyses of the oxide layers were performed by changing synchrotron radiation energy to estimate the oxide thickness. The native oxide layer was disappeared by thermal annealing up to 713 K for the V(111) surface. The oxide layers of the poly V and the VCrTa alloy, however, were remained even at 873 K. Although the oxides of V and Cr were disappeared, Ta oxides were remained. The re-arrangement of oxidation took place in the oxide layer of the VCrTa alloy by thermal annealing. The oxidation of Ta controlled oxide thickness in the VCrTa alloy. The formation of an artificial oxide layer could be controlled using supersonic oxygen molecular beams. 1. Introduction Hydrogen storage materials such as Vanadium compounds are important as candidates for fuel cells of automobiles [1]. In generally speaking, desorption and absorption of hydrogen molecules in the hydrogen storage materials take place through native oxide layers formed on the surface. Thus, it is important to study the nature of the oxide layer to control thermal desorption characteristics of hydrogen molecules. In order to study correlation between hydrogen desorption temperature and chemical bonding states of the oxide layer, photoemission spectroscopy with high brilliance and high energy-resolution synchrotron radiation (SR-XPS) has been applied for the analyses of the native oxide, its thermal instability, and the reformation of artificial oxides at the surfaces of single crystalline V(111), polycrystalline Vanadium and polycrystalline VCrTa alloy. 2. Experimental All experiments have been performed at the surface chemistry experimental station (SUREAC2000) of the BL23SU in the SPring-8 facilities [2]. The base vacuum pressure in this apparatus was less than 210 -8 Pa. Photoelectrons were detected by a concentric hemispherical analyzer with 5MCD. Photon energy used in this work was tuned from 592 eV to 1569 eV. The SR beam of 1247 eV was used for thermal instability and re-oxidation studies. The detection angle of photoelectrons was 30 degrees with respect to surface normal. Photoemission spectra for O-1s, C-1s, V-2p, V-3p, Cr-2p, Ta-4d and a wide scan were measured. Binding energy values of the inner shells were referred from a data book [3]. The thermal radiation from a Ta ribbon heater, which was set in the backside of sample, was used for sample heating. The thermal instability of native oxide layers was observed by the SR-XPS at room temperature after heating up to the destination temperature to avoid effects of a magnetic field generated in the Ta ribbon heater. The supersonic O 2 molecular beams (SSOMB) were used for the artificial oxides formation. Translational kinetic energy of the SSOMB is controllable from 0.02 eV to 2.3 eV by changing nozzle temperature and gas mixing ratio (O 2 /He/Ar). The energy value was calculated on the basis of the energy conservation law before and after adiabatic gas expansion from a nozzle orifice. After an appropriate O 2 beam dosage, photoelectron spectra were measured. The dosage and XPS measument cycle was continued until oxygen saturation. The O 2 flux density of the SSOMB was estimated from measurements of gas pressure increase in the reaction chamber, the gas mixing ratio, and the molecular beam spot size at the sample surface. 3. Results and Discussion 3.1 Analyses of Native Oxide by Changing Synchrotron Radiation Energy Photoemission spectra of V-2p and O-1s for the native oxide layer on the V(111) surface is shown in Fig. 1. A synchrotron radiation energy dependence Copyright (c) 2009 by The Surface Analysis Society of Japan

Upload: buidat

Post on 02-May-2018

220 views

Category:

Documents


1 download

TRANSCRIPT

Journal of Surface Analysis Vol.15 No.3 (2009) pp. 303-306 Yuden Teraoka et al. Synchrotron Radiation Photoemission Spectroscopy for Native Oxide Layer on V and VCrTa

−303−

Synchrotron Radiation Photoemission Spectroscopy for Native

Oxide Layer on Vanadium and VCrTa

Yuden Teraoka, Akitaka Yoshigoe, James Harries Japan Atomic Energy Agency, 1-1-1 Kouto, Sayo-cho, Sayo-gun, Hyogo 679-5148, Japan

[email protected]

(Received : December 29, 2008; Accepted: February 10, 2009)

In order to study correlation between oxide layers on hydrogen storage metals such as V(111), polycrystalline Vanadium, and VCrTa alloy and hydrogen desorption temperature, the surfaces covered by native oxides have been analyzed by photoemission spectroscopy using soft x-ray synchrotron radiation. Depth analyses of the oxide layers were performed by changing synchrotron radiation energy to estimate the oxide thickness. The native oxide layer was disappeared by thermal annealing up to 713 K for the V(111) surface. The oxide layers of the poly V and the VCrTa alloy, however, were remained even at 873 K. Although the oxides of V and Cr were disappeared, Ta oxides were remained. The re-arrangement of oxidation took place in the oxide layer of the VCrTa alloy by thermal annealing. The oxidation of Ta controlled oxide thickness in the VCrTa alloy. The formation of an artificial oxide layer could be controlled using supersonic oxygen molecular beams.

1. Introduction

Hydrogen storage materials such as Vanadium compounds are important as candidates for fuel cells of automobiles [1]. In generally speaking, desorption and absorption of hydrogen molecules in the hydrogen storage materials take place through native oxide layers formed on the surface. Thus, it is important to study the nature of the oxide layer to control thermal desorption characteristics of hydrogen molecules. In order to study correlation between hydrogen desorption temperature and chemical bonding states of the oxide layer, photoemission spectroscopy with high brilliance and high energy-resolution synchrotron radiation (SR-XPS) has been applied for the analyses of the native oxide, its thermal instability, and the reformation of artificial oxides at the surfaces of single crystalline V(111), polycrystalline Vanadium and polycrystalline VCrTa alloy. 2. Experimental

All experiments have been performed at the surface chemistry experimental station (SUREAC2000) of the BL23SU in the SPring-8 facilities [2]. The base vacuum pressure in this apparatus was less than 2☓10-8 Pa. Photoelectrons were detected by a concentric hemispherical analyzer with 5MCD. Photon energy used in this work was tuned from 592 eV to 1569 eV. The SR beam of 1247 eV was used for thermal instability and re-oxidation studies. The detection angle of photoelectrons was 30 degrees with respect to

surface normal. Photoemission spectra for O-1s, C-1s, V-2p, V-3p, Cr-2p, Ta-4d and a wide scan were measured. Binding energy values of the inner shells were referred from a data book [3].

The thermal radiation from a Ta ribbon heater, which was set in the backside of sample, was used for sample heating. The thermal instability of native oxide layers was observed by the SR-XPS at room temperature after heating up to the destination temperature to avoid effects of a magnetic field generated in the Ta ribbon heater.

The supersonic O2 molecular beams (SSOMB) were used for the artificial oxides formation. Translational kinetic energy of the SSOMB is controllable from 0.02 eV to 2.3 eV by changing nozzle temperature and gas mixing ratio (O2/He/Ar). The energy value was calculated on the basis of the energy conservation law before and after adiabatic gas expansion from a nozzle orifice. After an appropriate O2 beam dosage, photoelectron spectra were measured. The dosage and XPS measument cycle was continued until oxygen saturation. The O2 flux density of the SSOMB was estimated from measurements of gas pressure increase in the reaction chamber, the gas mixing ratio, and the molecular beam spot size at the sample surface. 3. Results and Discussion 3.1 Analyses of Native Oxide by Changing Synchrotron Radiation Energy

Photoemission spectra of V-2p and O-1s for the native oxide layer on the V(111) surface is shown in Fig. 1. A synchrotron radiation energy dependence

Copyright (c) 2009 by The Surface Analysis Society of Japan

Journal of Surface Analysis Vol.15 No.3 (2009) pp. 303-306 Yuden Teraoka et al. Synchrotron Radiation Photoemission Spectroscopy for Native Oxide Layer on V and VCrTa

−304−

was measured to estimate thickness of the layer. V-2p photoemission peaks contributed from bulk could be observed with photon energy larger than 795 eV so that the thickness might be about 2 nm assuming the detectable thickness was three times larger than escape depth. The O-1s photoemission spectrum consisted of at least two components. A shoulder structure seen in higher binding energy was changed to be minor in higher SR energy so that the component was surface sensitive.

505 510 515 520 525 530 535 540-0.2

0.0

0.2

0.4

0.6

0.8

1.0

1.2

1.4

1.6

1.8

2.0

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

V2p3/2 V2p1/2Oxides

O1s

591eV

687eV

795eV900eV

1010eV

1152eV1251eV1340eV1437eV1567eV

505 510 515 520 525 530 535 540-0.2

0.0

0.2

0.4

0.6

0.8

1.0

1.2

1.4

1.6

1.8

2.0

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

V2p3/2 V2p1/2Oxides

O1s

591eV

687eV

795eV900eV

1010eV

1152eV1251eV1340eV1437eV1567eV

A synchrotron radiation energy dependence of V-2p and O-1s photoemission spectra for the poly V surface is shown in Fig. 2. The profile is almost same as Fig. 1. V-2p peaks from the bulk could be observed from 795 eV so that the oxide thickness was estimated to be about 2 nm. The O-1s peak profile was also resembled with Fig. 1.

505 510 515 520 525 530 535 5400.0

0.5

1.0

1.5

2.0

Norm

ariz

ed

Photo

em

issi

on Inte

nsi

ty

Binding Energy/eV

V2p3/2 V2p1/2

OxidesO1s

1567eV

1437eV

1340eV

1246eV

1152eV

1010eV900eV

687eV591eV

795eV

505 510 515 520 525 530 535 5400.0

0.5

1.0

1.5

2.0

Norm

ariz

ed

Photo

em

issi

on Inte

nsi

ty

Binding Energy/eV

V2p3/2 V2p1/2

OxidesO1s

1567eV

1437eV

1340eV

1246eV

1152eV

1010eV900eV

687eV591eV

795eV

A synchrotron radiation energy dependence of V-2p and O-1s peaks for the VCrTa alloy is shown in Fig. 3. In contrast to the former two cases, the O-1s peak and chemically-shifted V-2p peaks are larger than those in Figs. 1 and 2. It implies that

further oxidation proceeds in this alloy comparing with the V(111) and the poly V. Indeed, V-2p peaks contributed from the bulk could be observed with photon energy larger than 1012 eV so that the oxide thickness might be about 2.4 nm. Although the O-1s peak profile showed an asymmetric shape tailing to the higher binding energy side, the surface sensitive component was not clearly observed.

505 510 515 520 525 530 535 540 5450.0

0.2

0.4

0.6

0.8

1.0

1.2

1.4

1.6

1.8

2.0

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

tyBinding Energy/eV

V2p3/2 V2p1/2

V Oxide

O1s

1571eV1440eV1343eV1248eV1154eV1012eV

901eV

795eV

505 510 515 520 525 530 535 540 5450.0

0.2

0.4

0.6

0.8

1.0

1.2

1.4

1.6

1.8

2.0

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

tyBinding Energy/eV

V2p3/2 V2p1/2

V Oxide

O1s

1571eV1440eV1343eV1248eV1154eV1012eV

901eV

795eV

It is interesting to investigate oxidation states of

Cr and Ta to consider the origin of thicker oxide layer formation. Synchrotron radiation energy dependences of Cr-2p and Ta-4d peaks are shown in Figs. 4 and 5. Cr-2p peaks contributed from bulk could be observed with photon energy larger than 1012 eV as well as V-2p. Ta-4d peaks, however, could be observed from 1440 eV so that the oxide thickness might be about 4 nm. These deeper oxygen atoms might be the origin of very small SR energy dependence of O-1s peak.

570 575 580 585 590 595 600-1.0

-0.5

0.0

0.5

1.0

1.5

2.0

2.5

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

Cr2pCr2p3/2 Cr Oxide

901eV

1012eV

1154eV

1248eV

1342eV

1440eV

1571eV

570 575 580 585 590 595 600-1.0

-0.5

0.0

0.5

1.0

1.5

2.0

2.5

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

Cr2pCr2p3/2 Cr Oxide

901eV

1012eV

1154eV

1248eV

1342eV

1440eV

1571eV

Fig. 1 Synchrotron radiation energy dependence of V-2p and O-1s peaks for a native oxide layer on V(111).

Fig. 2 Synchrotron radiation energy dependence of V-2p and O-1s peaks for a native oxide layer on poly V.

Fig. 3 Synchrotron radiation energy dependence of V-2p and O-1s peaks for a native oxide layer on VCrTa alloy.

Fig. 4 Synchrotron radiation energy dependence of Cr-2p peaks for a native oxide layer on VCrTa alloy.

Journal of Surface Analysis Vol.15 No.3 (2009) pp. 303-306 Yuden Teraoka et al. Synchrotron Radiation Photoemission Spectroscopy for Native Oxide Layer on V and VCrTa

−305−

210 220 230 240 250 260

0.0

0.5

1.0

1.5

2.0

Norm

aliz

ed

Photo

em

issi

on Inte

nsi

ty

Binding Energy/eV

Ta4d

Ta4d5/2 Ta Oxide

1571eV1440eV1343eV1248eV1154eV1012eV

901eV

795eV

210 220 230 240 250 260

0.0

0.5

1.0

1.5

2.0

Norm

aliz

ed

Photo

em

issi

on Inte

nsi

ty

Binding Energy/eV

Ta4d

Ta4d5/2 Ta Oxide

1571eV1440eV1343eV1248eV1154eV1012eV

901eV

795eV

3.2 Thermal Instability of Native Oxide

Thermal instability of the native oxide layer has been investigated by flash heating. Fig. 6 shows V-2p and O-1s variation depending on thermal annealing temperature ranging from 713 K and 1513 K for the V(111) surface. The bulk components of V-2p1/2 and V-2p3/2 peaks increased with decreasing O-1s peak. The O-1s peak decreased to be negligible even at 713 K. Small doublet peaks, however, remained even after heating up to 1513 K. The higher binding energy component is surface sensitive and the other peak corresponds to the main native oxide peak.

V2p3/2

V2p1/2

O1s

Native Oxide

505 510 515 520 525 530 535 540

0

5

10

15

20

25

30

35

40

45

Norm

aliz

ed P

hoto

em

issi

on

Inte

nsity

Binding Energy/eV

V2p3/2

V2p1/2

O1s

Native Oxide

V2p3/2

V2p1/2

O1s

Native Oxide

505 510 515 520 525 530 535 540

0

5

10

15

20

25

30

35

40

45

Norm

aliz

ed P

hoto

em

issi

on

Inte

nsity

Binding Energy/eV

The similar experiments were performed for the poly V. The results were indicated in Fig. 7. Although all photoemission spectra were not changed up to 573 K, the O-1s peak decreased and the bulk components of V-2p peaks increased at 673 K. The V-2p3/2 peak position was shifted slightly and a satellite peak structure was observed as well

due to high energy-resolution SR-XPS as shown in Fig. 8. The peak shift may be attributed to a structure reconstruction at the surface by surface melting. And the satellite structure may correspond to sub-oxides because oxygen coverage decreased with increasing temperature. The O-1s peak disappeared completely at 1273 K. A clean surface could be obtained only by thermal annealing in the ultra high vacuum condition.

505 510 515 520 525 530 535 5400

10

20

30

40

50

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

300K

673 K

773 K

873 K

1273 K

300K

1273K

V2p3/2

Oxides

V2p1/2O1s

505 510 515 520 525 530 535 5400

10

20

30

40

50

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

300K

673 K

773 K

873 K

1273 K

300K

1273K

V2p3/2

Oxides

V2p1/2O1s

300K

673 K

773 K

873 K

1273 K

300K

1273K

V2p3/2

Oxides

V2p1/2O1s

510 511 512 513 514 5150

10

20

30

40

50

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

Sub-oxides

V2p3/2

1273K

873K

773K

673K

300K

510 511 512 513 514 5150

10

20

30

40

50

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

Sub-oxides

V2p3/2

1273K

873K

773K

673K

300K

In contrast to the single element V, thermal instability of the native oxide layer of the VCrTa alloy was complicated. Although V peaks from bulk grew with increasing temperature as seen in the single element V cases, the O-1s peak was remained as shown in Fig. 9.

Thermal annealing effects for Cr-2p peaks are shown in Fig. 10. Chemically-shifted oxide peaks were disappeared and bulk components grew to be main peaks as seen in the V-2p case. These results indicate that Cr-O bonds are broken and metal Cr or its alloy is segregated on the surface. On the other hand, chemically-shifted components of Ta-4d

Fig. 6 Thermal annealing effects for V-2p and O-1s peaks of a native oxide layer on V(111) by heating at 713 K to 1513 K observed with the photon energy of 1247 eV.

Fig. 5 Synchrotron radiation energy dependence of Ta-4d peaks for a native oxide layer on VCrTa alloy.

Fig. 7 Thermal annealing effects for V-2p and O-1s peaks of a native oxide layer on poly V observed with the photon energy of 1247 eV.

Fig. 8 Thermal annealing effects for V-2p3/2 peak of a native oxide layer on poly V observed with the photon energy of 1247 eV.

Journal of Surface Analysis Vol.15 No.3 (2009) pp. 303-306 Yuden Teraoka et al. Synchrotron Radiation Photoemission Spectroscopy for Native Oxide Layer on V and VCrTa

−306−

peaks were not disappeared by heating as shown in Fig.11. Ta-O bonds are still remained even up to 873 K. These facts imply that oxygen atoms bonding with V and Cr may be transferred to Ta.

500 505 510 515 520 525 530 535 540 5450.5

1.0

1.5

2.0

2.5

3.0

3.5

4.0

Norm

aliz

ed

Photo

em

issi

on Inte

nsi

ty

Binding Energy/eV

V2p3/2

V2p1/2

O1s

873K

773K

673K

473K

573K

300K

500 505 510 515 520 525 530 535 540 5450.5

1.0

1.5

2.0

2.5

3.0

3.5

4.0

Norm

aliz

ed

Photo

em

issi

on Inte

nsi

ty

Binding Energy/eV

V2p3/2

V2p1/2

O1s

873K

773K

673K

473K

573K

300K

570 575 580 585 590 595

1.0

1.2

1.4

1.6

1.8

2.0

Norm

aliz

ed

Photo

em

issi

on Inte

nsi

ty

Binding Energy/eV

Cr2p773K

673K

573K

473K

300K

873K

Cr Oxide

Cr2p3/2 Cr2p1/2

570 575 580 585 590 595

1.0

1.2

1.4

1.6

1.8

2.0

Norm

aliz

ed

Photo

em

issi

on Inte

nsi

ty

Binding Energy/eV

Cr2p773K

673K

573K

473K

300K

873K

Cr Oxide

Cr2p3/2 Cr2p1/2

210 220 230 240 250 260

1.0

1.5

2.0

2.5

3.0

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

Ta4d

873K

773K

673K

573K

473K

300K

Ta4d5/2 Ta4d3/2

Ta Oxide

210 220 230 240 250 260

1.0

1.5

2.0

2.5

3.0

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

Ta4d

873K

773K

673K

573K

473K

300K

Ta4d5/2 Ta4d3/2

Ta Oxide

3.3 Artificial Oxide Formation at V(111) The clean surfaces of V(111) and poly V, formed

by heating up to 1273 K, were irradiated by SSOMB with 2.3 eV until oxygen saturation after cooling down to room temperature. In both cases, similar oxide layers were formed. The spectral change of V-2p and O-1s for the V(111) surface is shown in Fig. 12. The bulk V-2p peak intensity was larger than that for the native oxide layer. The bulk sensitive component of O-1s peak grew to be major. Although the reason why the differences of V-2p and its oxide peaks between the native oxide and the artificial oxide was now under investigation, it was confirmed that the oxidation could be controlled by SSOMB in the present preliminary experiments.

505 510 515 520 525 530 535 540

0

5

10

15

20

25

30

35

40

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

V2p3/2

V2p1/2

O1s

Native Over-Layer

Max. O2 dose : 4.9x1017 molecules・cm-2

505 510 515 520 525 530 535 540

0

5

10

15

20

25

30

35

40

Norm

aliz

ed P

hoto

em

issi

on Inte

nsi

ty

Binding Energy/eV

V2p3/2

V2p1/2

O1s

Native Over-Layer

Max. O2 dose : 4.9x1017 molecules・cm-2

4. Acknowledgements

This work has been supported by New Energy and Industrial Technology Development Organization (NEDO) under "Advanced Fundamental Research Project on Hydrogen Storage Materials". 5. References [1] H. Arishima, F. Takahashi, T. Ebisawa, H. Itoh

and T. Kabutomori, J. Alloy and Comp. 405, 356 (2003).

[2] Y. Teraoka, A. Yoshigoe, and K. Moritani, Electrical Engineering in Japan 164(3), 60 (2008).

[3] J. Emsley, The Elements, 3rd Edn., Oxford University Press, Oxford (1998). Fig. 11 Thermal annealing effects for Ta-4d peaks of a

native oxide layer on VCrTa alloy observed with the photon energy of 1247 eV.

Fig. 10 Thermal annealing effects for Cr-2p peaks of a native oxide layer on VCrTa alloy observed with the photon energy of 1247 eV.

Fig. 9 Thermal annealing effects for V-2p and O-1s peaks of a native oxide layer on VCrTa alloy observed with the photon energy of 1247 eV.

Fig. 12 Artificial oxide formation at V(111) surface by irradiation of supersonic oxygen molecular beams with translational energy of 2.3 eV. The V-2p peaks decreased and in turn O-1s peak increased during O2 beam irradiation up to 4.9☓1017 molecules ・ cm-2 until saturation. The photon energy was 1247 eV.