spe distinguished lecturer program - society of … agenda • problem description • corrosion...
TRANSCRIPT
![Page 1: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/1.jpg)
1
SPE Distinguished Lecturer Program
Primary funding is provided by
The SPE Foundation through member donations and a contribution from Offshore Europe
The Society is grateful to those companies that allow their professionals to serve as lecturers
Additional support provided by AIME Society of Petroleum Engineers Distinguished Lecturer Program www.spe.org/dl
![Page 2: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/2.jpg)
Near Surface External Casing Corrosion; Cause, Remediation and Mitigation
Jerry Dethlefs ConocoPhillips Company
Society of Petroleum Engineers Distinguished Lecturer Program www.spe.org/dl
![Page 3: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/3.jpg)
3
Agenda
• Problem Description
• Corrosion Mechanism
• Repair Process – Excavation – Patch
• Mitigation Process – Sealant
• Summary and Conclusions
Alaska North Slope
![Page 4: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/4.jpg)
4
Kuparuk Operations • Approximately 1200 wells • Field startup in 1981 • First Surface Casing (SC) corrosion noted in 2000 • By 2005 over 25 wells with SC leaks
![Page 5: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/5.jpg)
5
The Problem
• Escalating rate of SC failures – Holes near surface from 0 to 25’+ – Detected by leaks at surface
• SC is a well barrier – Well integrity issues – Production impacts
• What is the cause and long term cost impact?
![Page 6: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/6.jpg)
6
Surface Casing Corrosion
![Page 7: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/7.jpg)
7
Investigation
SC corrosion NOT related to:
– Age of well – Electrical stray currents – Surface location
• There ARE correlations with: – Design
• Number of casing strings – Type of service
• Temperature correlation
Surface Casing Leaks - Year of Completion
0
1
2
3
4
5
6
7
8
1983
1985
1987
1989
1991
1993
1995
1997
1999
2001
Year Completed
Wel
ls w
ith S
C L
eaks
![Page 8: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/8.jpg)
8
Findings • Conducted field tests with corrosion consultant
• Root cause: Primary cement procedure combined with Arctic cement blends
Mechanism: • Repeated wetting of cement with oxygenated water • Cement breakdown = corrosive fluid • Add heat from production • Galvanic and thermo-galvanic cells • SC becomes sacrificial anode • Conductor becomes cathode
![Page 9: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/9.jpg)
9
Corrosive Fluid Oxygenated water becomes an electrolyte in the
annulus due to components of degraded cement
Electrolyte Resistivity: The lower the resistance value, the easier it conducts electricity and is more corrosive. Resistivity (Ohm-cm) General Category Less than 500 Extremely Corrosive 501-1,000 Very Corrosive 1,001-5,000 Corrosive 5,001-10,000 Moderate-Mildly Corrosive Above-10,000 Normally not significant
Source: Farwest Corrosion Control Report 6731, J. Bollinger
![Page 10: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/10.jpg)
10
Test Samples From One Well Material & Source Resistivity Classification Cellar Water 1,020 Corrosive Cement ( Dry) 400,000 Not significant Cement (Saturated) 38 Extremely Corrosive Soil Adjacent cellar (Dry) 58,000 Not significant Soil Adjacent cellar (Sat) 3,700 Corrosive
Source: Farwest Corrosion Control Report 6731 J. Bollinger
![Page 11: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/11.jpg)
11
Well Construction
Surface Casing ~2,500’ TVD Cemented to surface
Cement fallback
• Fluid losses
• Fracture zones
• Voids
• 0’ to > 100’
Cellar box
Conductor @ 120’ RKB Cemented to surface
Arctic Set cement 15% Salt and Gypsum
![Page 12: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/12.jpg)
12
Galvanic Cell in Annulus (Cross Section)
Corrosive water in annulus
Salt Bridge(Cement Additives)
Anode(Surface Casing)
Cathode (Conductor Casing)
Oxidation Reduction
Electrons
GALVANIC CELL
Primary cement top
High Temp
Low Temp
Corrosion
Surface Casing Conductor
![Page 13: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/13.jpg)
13
Heat Increases Corrosion Rate Single Casing Completion with Hot Water Injection* • One less annulus to insulate from permafrost • Higher Temperature Gradient = Faster Thermo-Galvanic
Corrosion
Thermo-Galvanic Corrosion
• Caused by thermal gradient
• Similar effect as galvanic corrosion
• Anodic and cathodic areas are formed
• Corrosion attack will develop
Source: Farwest Corrosion Control Report 6731, J. Bollinger
*‘A’ annulus and conductor; no ‘B’ annulus
![Page 14: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/14.jpg)
14
Primary Cement Blend Surface Casing Cement • Good cement minimizes corrosion • Light weight cement to reduce hydrostatic head • Designed to set prior to freezing in permafrost zone
Additives = Complications • +/- 15% Salt for Freeze Point Depression
– Salt Water = Higher Corrosion Rates • Gypsum for Heat of Hydration
– Gypsum = Plaster of Paris • Degrades Rapidly in Water
• Lead slurry contaminated during displacement
![Page 15: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/15.jpg)
15
To Initiate Corrosion: Just add oxygenated water from
snow melt or rain--
Oxygen Enriching Algae in Water
And repeat year after year!
Water Level Marks in Culvert
![Page 16: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/16.jpg)
16
Remediation Process • Excavation • Preparation • Patch • Important:
– Perform risk assessment – Wells require safe-out – Follow HSE guidelines
![Page 17: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/17.jpg)
17
Excavation Methods Shallow – Vacuum Removal
![Page 18: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/18.jpg)
18
Excavation Methods Moderate – Backhoe & Scaffold
![Page 19: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/19.jpg)
19
Excavation Methods Deep – Backhoe & Trench Box
![Page 20: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/20.jpg)
20
Multiple Well Excavation
![Page 21: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/21.jpg)
Current Approach
• Minimal cellar
• Up to 8’ deep
• Low cost option
![Page 22: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/22.jpg)
22
Conductor Removal Methods Torch
![Page 23: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/23.jpg)
23
Conductor Removal Methods Casing Window Cutter
![Page 24: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/24.jpg)
24
Cement Sheath Removal Conductor
![Page 25: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/25.jpg)
25
Shallow Repair Sequence
• Buff or sandblast SC
• Ultrasonic Thickness (UT) inspection
• Engineered patch
![Page 26: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/26.jpg)
26
Shallow Repair Sequence Install SC sleeve – typically split casing
![Page 27: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/27.jpg)
27
Shallow Repair Sequence Sleeve installed and welded
![Page 28: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/28.jpg)
28
Shallow Repair Sequence Corrosion protection installed over sleeve
![Page 29: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/29.jpg)
29
Shallow Repair Sequence Re-install Conductor
Fill with cement and top with sealant
![Page 30: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/30.jpg)
30
Corrosion Mitigation Process
• Existing wells: – Seal water entrance paths
• Weld or plug conductor holes • Top-fill with cement to near surface • Top with dielectric sealant
• New wells - Drilling – Improve cementing practice
• Cement to near surface • Top with dielectric sealant
![Page 31: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/31.jpg)
31
Job of Sealants • Seal annulus from water and oxygen
– Even if completely submersed • Suitable for wide temperature fluctuations • Environmentally benign • Should be removable • Should remain in place
– No “Projectile” with deeper Leak • Should be replenishable
![Page 32: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/32.jpg)
32
Sealant Properties • “Grease-like” product • Dielectric properties • Non hardening co-polymer • Excellent corrosion
performance • Provides protective film • Densified with zinc dust
– Heavier than water • Best performance
Pipe immersed in aerated salt solution covering insulation for 2 Years Courtesy of Denovus
![Page 33: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/33.jpg)
33
Treatment Temperature
• Sealant 115 to 130 F • Will not burn workers • Sufficient to self level • Will not overflow when at operating temperature
![Page 34: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/34.jpg)
34
Treatment Overview
SC ~ 2,500’ TVD
Cement fallback
• Fluid losses
• Fracture zones
• Voids
Raise cement top “Top Job” with hose &
low pressure pump
Top with sealant
(1-2’ typical)
![Page 35: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/35.jpg)
35
What Sealant Looks Like
![Page 36: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/36.jpg)
36
Project Status
As of July 2010: • 56 casing failures known or suspected
• 45 excavations and patches completed
• 1133 wells sealant treated
![Page 37: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/37.jpg)
37
Patch Economics
• Cost < 6% of rig workover repairs
• Savings > $65,000,000 – Over 8-year period compared to using rotary rig – Assuming 50% of wells were “economic” to repair
• More wells remain in service due to robust patch economics
![Page 38: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/38.jpg)
Sealant Mitigation
• Treat remaining wells in Kuparuk and satellite fields
• New wells treated after release by Drilling
• Other North Slope Operators adopting program
• Applicable in many global locations
38
![Page 39: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/39.jpg)
39
Conclusion • SC corrosion cause identified
• SC repairs on-going
• Mitigation in progress
• Improved cement procedures for new wells
• A non-traditional, non-rig repair can be a safe, cost-effective alternative
![Page 40: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/40.jpg)
Application
• Offshore locations – Saltwater exposure
• Onshore – Cement additives – Shallow surface water sources – Production fluids release – Well servicing fluid exposure
![Page 41: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/41.jpg)
41
Thank you!
Questions?
![Page 42: SPE Distinguished Lecturer Program - Society of … Agenda • Problem Description • Corrosion Mechanism • Repair Process – Excavation – Patch • Mitigation Process – Sealant](https://reader031.vdocuments.site/reader031/viewer/2022022509/5ad4ce0a7f8b9a0d2d8ce261/html5/thumbnails/42.jpg)
42
Based on: SPE-100432-PP Near Surface Casing Corrosion in
Alaska; Cause and Mitigation Jerry Dethlefs, Curtis Blount, ConocoPhillips and
John Bollinger, Farwest Corrosion Company Contributions by ConocoPhillips Alaska Wells Group
• Published: – SPE Drilling & Completion Journal, December 2008, Volume 23,
Number 4
• Reference: – SPE 50967 Corrosion Problems in Below-Grade Wellhead Equipment
and Surface Casings
• Special thanks: – MJ Loveland and Perry Klein, ConocoPhillips Alaska Wells Group