Welding Procedure Guide © Copyright 2008 CWB Group - Industry Services ® An easy to follow guide covering the preparation of welding procedure data sheets

Upload: cmontminy

Post on 29-Nov-2014

1.259 views

Category:

Documents


12 download

TRANSCRIPT

Page 1: CWB Welding Procedure Guide

Welding

ProcedureGuide

© Copyright 2008 CWB Group - Industry Services

®

An easy to follow guide covering the preparation of welding procedure data sheets

Page 2: CWB Welding Procedure Guide

© Copyright CWB Group - Industry ServicesRevised September 2008

All rights reserved.

CWB Group1-800-844-6790

www.cwbgroup.org

®

Page 3: CWB Welding Procedure Guide

ii© Copyright CWB Group - Industry Services

®

TABLE OF CONTENTS

1.0 Introduction 2

2.0 Welding Engineering Standards 3

3.0WeldingProcedureSpecification(WPS) 3

4.0WeldingProcedureDataSheet(WPDS) 4

4.1 BLOCK1(GeneralInformation) 6

4.2 BLOCK2(Processinformation) 7

4.3 BLOCK3(Jointinformation) 8

4.4 BLOCK4(Technicaldata) 11

4.5 BLOCK5(Jointpreparation) 13

4.6 BLOCK6(BaseandFillermaterial) 14

4.7 BLOCK7(Weldingdetails) 16

4.8 BLOCK8(Finalremarks) 20

5.0 Submission Of Welding Procedures 23

6.0 Review And Approval Of Welding Procedures 24

7.0 Sample Welding Procedure Data Sheets 26

Page 4: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services

Page 5: CWB Welding Procedure Guide

Page 1© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

1.0 Introduction

ThisguidehasbeenpreparedtoassistweldingpersonnelwiththepreparationofweldingproceduresrequiredaspartoftheircompanycertificationtoCSAStandardsW47.1,W47.2andW186.

Thefollowingthreedocumentswillbedescribed:

(a)WeldingEngineeringStandards(Note:OnlyrequiredforW47.2)

(b)WeldingProcedureSpecifications

c)WeldingProcedureDataSheets

Therewillbeabriefdescriptionofthefirsttwodocuments;however,thisguidewillfocusonthepreparationof welding procedure data sheets. Each item on the welding procedure data sheet will be described and guidance will be provided to complete each section.

Page 6: CWB Welding Procedure Guide

Page 2 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

2.0 Welding Engineering Standards

Welding engineering standards cover the design of welded joints encountered by the fabricator and

prepared primarily for the fabricator’s engineering and drafting personnel.

Theweldingengineeringstandardstypicallyinclude:

(a)Illustratedprofilesofeachtypicaljointintendedforuse,showing:

(i)Thetypeofjoint(eg,butt,lap,tee,corner,edge);

(ii)Thetypeofweld;

(iii)Thegeometryofthepreparationandfit-up;

(iv)Thestandardweldingsymbol;

(v)Therangeofthickness;and

(b)Minimumpermissiblesizesoffilletandpartialpenetrationgroovewelds.

Welding symbols shall be as shown in AWS Standard A2.4.

Sample welding engineering standards are available on our website www.cwbgroup.org

3.0 WeldingProcedureSpecification(WPS)

AllcompaniesapplyingorcertifiedtoCSAStandardsW47.1,W47.2orW186arerequiredtoprepareand

submitweldingprocedurespecificationstotheCWBforacceptance.

Aweldingprocedurespecification(WPS)setsbroadguidelinesfortheshopandfieldweldingpracticeofthe fabricator for each anticipated combination of essential variables. Welding parameters and ranges are specifiedandusedtopreparetheassociatedweldingproceduredatasheets.

Page 7: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 3© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

Thecompanyshallhaveweldingprocedurespecificationsforeachweldingprocessinuse,outliningthegeneral welding procedure to be followed in the construction of weldments built in accordance with the governingdesignormanufacturingstandard,orboth.WeldingprocedurespecificationssubmittedforacceptanceshouldcoverasaminimumtheitemsspecifiedinAppendixDofCSAStandardW47.1orAppendixAofCSAStandardW47.2,asapplicable.Eachweldingprocedurespecificationshallincludeapplicableessentialvariables.AllweldingprocedurespecificationsshallbesubmittedtotheBureauforacceptance and when stamped as accepted shall be considered as registered with the Bureau.

Sampleweldingprocedurespecificationsareavailableonourwebsitewww.cwbgroup.org

4.0 WeldingProcedureDataSheet(WPDS)

Aweldingproceduredatasheet(WPDS)isadocument,usedinconjunctionwithaWPS,detailingtheweldingparametersandrangesforweldingaspecificjoint,overarangeofthicknessesandweldsizes,asillustratedonthedatasheet.ThefollowingisthestandardweldingproceduredatasheetformsuggestedbytheCWB,however,otherweldingproceduredatasheetformatsmaybeused.Eachitemonthedatasheetwill be described and guidance on the completion of the form will be given. Common errors in completing theformwillbeidentified.

Page 8: CWB Welding Procedure Guide

Page 4 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

Page 9: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 5© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

4.1 BLOCK1(GeneralInformation)

Companynameandaddress

Enter the complete company name and address in this section. If the data sheets are to be used by twoormorecertifiedplantswithinthesamecompanytheapplicableplantsneedtobeidentifiedinthedocumentation submitted.

WPDS No.

Eachcompanyshouldhaveitsownmethodofnumberingweldingproceduredatasheets.Thiscanrangefromarelativelysimpleconsecutivenumbersystemtoonethatidentifiestheprocess,position,groovetypeand electrode. Each welding procedure data sheet number should be unique so that the WPDS can be easilyreferencedonproductionschedules,workorders,shopdrawingsetc.

Date and Revision

Enter the date the welding procedure data sheet was prepared and the revision number.

ReferenceStandards

Someweldingstandardsthatmaybereferencedare:

W47.1–CertificationofCompaniesforFusionWeldingofSteel

W59–WeldedSteelConstruction(MetalArcWelding)

W186 – Welding of Reinforcing Bars in Reinforced Concrete Construction

W47.2–CertificationofCompaniesforFusionWeldingofAluminum

W59.2 – Welded Aluminum Construction

AWSD1.1 – Structural Welding Code - Steel

AWSD1.3 – Structural Welding Code – Sheet Steel

AWSD1.6 – Structural Welding Code – Stainless Steel

AcommoncombinationisW47.1andW59.Forcertifiedcompanies,theremustalwaysbeacertificationstandardstated(eg.W47.1,W47.2,W186)plusa“Construction”standard(eg.W59,W59.2,D1.3,D1.6).

Page 10: CWB Welding Procedure Guide

Page 6 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

ReferenceWPS

Recordtheweldingprocedurespecificationnumberthatappliestothisdatasheet.

SomecommonmistakeswithBlock1:

Thecompanynameandaddressarenotcompleted.•

Morethanonedatasheethasthesameidentificationnumber.•

Noreferencecodeisspecified.•

Referencecodesarespecifiedthathavedifferentqualificationrulesandessentialvariables.For•exampleW59andD1.3.

4.2 BLOCK2(Processinformation)

Welding Processes

Theweldingprocesstobeusedshouldbespecifiedinthissection.Iftwoweldingprocessesareusedtoweldthejointtheycanbeeachbeenteredintheareasidentified“1”and“2”.Someofthecommonprocessesusedarelistedbelowwiththeircorrespondingletterdesignations:

Process Letter Designation

ShieldedMetalArcWelding SMAW

GasMetalArcWelding GMAW

FluxCoredArcWelding FCAW

MetalCoredArcWelding MCAW

GasTungstenArcWelding GTAW

Submerged Arc Welding SAW

Plasma Arc Welding PAW

Electroslag Welding ESW

Electrogas Welding EGW

Stud Welding SW

Theletterdesignationmaybeusedtoidentifytheprocess.

FulldetailsaboutthevariousweldingprocessescanbefoundintheCWBmodules.

Page 11: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 7© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

Pulsed

Ifpulsedcurrentisusedcheckthisbox.Entertherootmeansquare(RMS)currentinblock7andthepeakandbackgroundcurrentintheremarkssectionofblock8.Thepulsedpowersourcebrand,modelnameandtheapplicableprogramnumbershouldalsobenotedintheremarkssection(Block8).

Shielding Gas type

Record the complete generic composition or gas trade name as shown on the label on the gas cylinder.

Use of the generic composition is advantageous as it allows the user to change brands of shielding gas with the same composition with no required changes to the WPDS.

Note:Ifthetradenameisused,achangetoanotherbrandname,evenifitisofidenticalcomposition,willrequire revised data sheets.

Thegasmanufacturer/suppliermaybeabletoprovideyouwiththegenericcomposition.Forgasmetalarcwelding,thewireisclassifiedusing100%CO2;however,argon-oxygen-carbondioxidecombinationsmaybeusedbasedontheoxygenequivalent.

ForfulldetailsofgascombinationsrefertoCSAStandardW48.

SomecommonmistakeswithBlock2:

Noweldingprocessspecified•

Nogascompositionspecified•

Gasnotcertifiedwiththefillermaterial•

4.3 BLOCK3(Jointinformation)

Positions

PositionsshownonthedatasheetshouldbetheproductionpositionclassifiedasFlat(F),Horizontal(H),Vertical-Up(V-U),VerticalDown(V-D)orOverhead.

Numberandlettercombinationsarealsousedtodesignateeachweldingpositionforquickreference.TheletterGstandsforgrooveweld,letterFforfilletweld.Thenumbers1,2,3and4correspondtoflat,horizontal,verticalandoverheadpositionsrespectively.Fortheverticalpositionindicateiftheprogressionis vertical up or vertical down.

Page 12: CWB Welding Procedure Guide

Page 8 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

Inactualshopfabricationweldingcanbeinanyintermediateposition.FordetailedinformationonthedefinitionofthevariousweldingpositionspleaseconsultAppendixEofCSAStandardW59,WeldedSteelConstruction(MetalArcWelding)orAWSA3.0,StandardWeldingTermsandDefinitions.

Processmode(manual,semi-automatic,machineandauto)

Oneofthefourprocessmodesshouldbecheckedinthissectionbasedonthefollowingdefinitions.Donotenter more than one process mode unless multiple processes are used.

Manualwelding.Weldingwiththetorch,gunorelectrodeholderheldandmanipulatedbyhand.Accessoryequipment,suchaspartmotiondevicesandmanuallycontrolledfillermaterialfeedersmaybeused.AnexampleisSMAWorGTAW.

Semi-automaticwelding.Manualweldingwithequipmentthatautomaticallycontrolsoneormoreoftheweldingconditions.ExamplesareFCAW,GMAW

Machinewelding(mechanizedwelding).Weldingwithequipmentthatrequiresmanualadjustmentoftheequipmentcontrolsinresponsetovisualobservationofthewelding,withthetorch,gunorelectrodeholderheldbyamechanizeddevice.SAWisanexample.

Automatic welding. Welding with equipment that requires only occasional or no observation of the welding andwithnomanualadjustmentoftheequipmentcontrols.Anexampleisaroboticapplication.

Jointtype

Checkthebox(s)toindicatethejointtype.Thefivebasictypesarebutt,tee,corner,lapandedge.

Fordefinitionsanddetailsofjointtype,pleaseconsultCWBModule2,EngineeringDrawings,BasicJointsand Preparation for Welding.

Page 13: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 9© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

Penetration(complete,partial,ETT)

Thedepthofpenetrationofagrooveweldneedstobeidentified.

Acompletejointpenetrationgrooveweldisdefinedasoneinwhichtheweldmetalextendsthroughthejointthickness.Thiscanbeachievedwithorwithoutbacking.Ifcompletejointpenetrationisachievedtheboxmarked“Complete”shouldbechecked.

Apartialjointpenetrationgrooveweldisoneinwhichincompletejointpenetrationexists.Ifthisisthecasetheboxmarked“Partial”shouldbecheckedandtheeffectivethroatthickness(ETT)shouldbedimensionedinthespaceprovided.TheETTmaybespecifiedasapercentageofT,eg.ETT=0.75T.Table4-3ofCSAStandardW59showsminimumgroovedepthsforpartialjointpenetrationgrooveweldsbasedonthethicknessofthepartsandthegrooveangleattheroot.Verifythattheserequirementsaremet.

Fillet

Theboxmarked“fillet”shouldbecheckediftheweldisaweldofapproximatelytriangularcrosssectionjoiningtwosurfacesapproximatelyatrightanglestoeachotherinalap-joint,T-jointorcornerjoint.Jointswithagrooveanglegreaterthan135degreesorlessthan30degreesrequiregreaterdetailinthesketch(definedasskewedjoints).RefertoW59Clause4.5formoredetail.

Backing(materialandthickness)

Backingisamaterialordeviceplacedagainstthebacksideofthejointadjacenttothejointroottosupportand shield molten weld metal.

Permanentbackingisdesignedtoremaininplaceaspartofthefinishedweld.

Backingsusedfortheweldingofsteelsuptoandincluding480MPa(70ksi)minimumspecifiedtensilestrength may be any of the steels listed in clauses 11.2.1 and 12.2.1 of CSA Standard W59.

W59requiresthatbackingsusedfortheweldingofsteelsofover480MPa(70ksi)minimumspecifiedtensile strength and shall be of the same material as the base material.

Ifsteelbackingisusedenterthematerialandthicknessofbackinginthespaceprovided

Non-permanentbackingscanbemadefrommaterialssuchasceramic,copperorflux.Iftheyareusedenterthematerial,typeandformofthebackinginthespaceprovided.

Page 14: CWB Welding Procedure Guide

Page 10 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

Backgouging(Yes/No,Method,Depth)

Backgougingistheremovalofweldmetalandbasemetalfromtheweldrootsideofaweldedjointtofacilitatecompletefusionandcompletejointpenetrationuponsubsequentweldingfromthatside.Methodsincludegrindingtosoundmetal(GTSM),aircarbonarcandplasma.

BackgougingshouldproduceagroovecontoursubstantiallyconformingtotheappropriateprequalifiedsingleU-jointinClause10ofCSAStandardW59,anditsdepthshouldbeadequatetoensurecompletepenetration into the previously deposited weld metal for the welding process to be used.

Ifbackgougingisused,thebackgougingboxshouldbechecked.Themethodusedandthedepthidentified.

SomecommonmistakeswithBlock3:

Noweldingpositionspecified.•

Incorrectweldingpositionspecified.Forexample,thedrawingshowshorizontal(2For2G)butposition•says“Flat”.

Progression of welding not shown for Vertical. •

PartialjointpenetrationspecifiedwithETT=T•

NoETTspecifiedforpartialjointpenetration•

Bothfilletandpartialboxesarechecked(Completeorpartialjointpenetrationonlyapplytogroove•welds)

4.4 BLOCK4(Technicaldata)

Electrode extension

Theelectrodeextensionforthegasmetalarcwelding,fluxcoredarcwelding,submergedarcweldingprocessesisthelengthofelectrodeextendingbeyondtheendofthecontacttip.

Theelectrodeextensionforthegastungstenarcweldingandplasmaarcweldingprocessesisthelengthofelectrodeextendingbeyondtheendofthecollett.

Entertheelectrodeextensioninthissection.Donotleaveitblank.IftheinformationrequesteddoesnotpertaintotheweldingprocessusedinsertN/A(NotApplicable)e.g.SMAW.

Page 15: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 11© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

Nozzlediameter

Thegasnozzleisthedeviceattheexitendofthetorchorgunthatdirectsshieldinggasingasshieldedprocesses.Enterthediameterofthisnozzleinthespaceprovided.Ifitdoesnotapply(eg.non-gasshieldedprocesses),enterN/A.

Fluxclassification

Forthesubmergedarcwelding(SAW)processthefluxclassificationorfluxtradenameshouldbeenterede.g.EM12Korthefluxtradename.Thisinformationcanbeobtainedfromthelabelonthebagofflux.Ifyouenterthefluxtradenameanddecidelatertochangethefluxthedatasheetwillneedtoberevised.Thegenericclassificationispreferred.

Tungstenelectrodes(type,dia.)

ThetungstentypeanddiameterusedshouldbespecifiedfortheGTAWprocess.ForotherprocessesenterN/A.Thechoiceofthetypeandsizeoftungstenelectrodeforaparticularapplicationdependsontheoperating current and current type.

Common tungsten types are listed below.

AWSCLASSIFICATION COMMONNAME COLOUR CODEEWCe-2 2%CeriatedTungsten OrangeEWLa-1 1%LanthanatedTungsten BlackEWTh-1 1%ThoriatedTungsten YellowEWTh-2 2%ThoriatedTungsten RedEWZr-1 1%ZirconiatedTungsten BrownEWG Other-NeedstobeSpecified Gray

Cleaning procedures

Enterthecleaningproceduresused.Thisisparticularlyimportantfortheweldingofaluminumalloysbecauseachangeincleaningmethodisconsideredanessentialvariable.Fulldetailsofthecleaningprocedureusedshouldbeincludedinthecorrespondingweldingprocedurespecification.

CSA W186 Rebar splice type.

ThissectionisonlyusedforweldingproceduredatasheetsforCSAStandardW186-ReinforcingBars.

ThetypesidentifiedinCSAStandardW186are:

direct splice•

indirect splice•

lap splice•

rebar to structural member•

Page 16: CWB Welding Procedure Guide

Page 12 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

SomecommonmistakeswithBlock4:

Electrodestickoutnotspecified•

Incompleteornocleaningproceduresspecified•

4.5 BLOCK5(Jointpreparation)

JointConfigurationandPass/Layersequence

Asketchofthejointconfigurationwiththeweldingsymbolandatypicalsequenceofthelayersandpassesshouldbeincludedinthissectionoftheform.Itisrecommendedthatthesketchbedrawninthecorrectwelding postion.

Thejointconfigurationshouldincludethefollowinginformation:

thicknessofparts•

root opening•

root face•

bevel angle•

groove angle•

depth of preparation•

radius(forHSS)•

diameter(forsolidbars/tubing/pipe)•

effectivethroatthickness(ETT)•

SomecommonmistakeswithBlock5:

Missingdetailssuchasrootfaceorland(Rf),Rootgaporopening(G),grooveangle(Θ),radius•

Nonpre-qualifiedmaterialthickness.Ex:0.9mmGMAWwireisnotpre-qualifiedforgrooveweldswith•amaterialthicknessgreaterthan12mm.

Page 17: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 13© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

4.6 BLOCK6(BaseandFillermaterial)

Identificationofbasematerial(specificationandgrade,thicknessordiameter,specialrequirements)

Obtainacopyofthemilltestcertificateoranyotherdocumentfromthematerialsupplierthatshowsthespecificationandgradeofthebasematerials.Recordthecompletematerialspecificationsandgradesontheweldingproceduredatasheets.Checkwithyourpurchasingagent.

Thefollowingaresomeexamplesofcorrectandincorrectmaterialdesignations:

Incorrect Correct

44W CSA Standard G40.21 Grade 300W

A572 ASTMA572Grade50

Gr. 400 Rebar CSA Standard G30.18 Grade 400W

Notethatmanymaterials,especiallyASTMmaterials,haveagradedesignationwhichmustbeincluded.

Anothercommonmethodtodesignatematerialsondatasheetsistousesteelgroupssuchas“Steelsingroups1,2and3ofTable11-1/12-1ofCSAStandardW59.Thisisadvantageousasitensuresawiderange of materials are covered.

Identificationoffillermaterial(process,tradename,classification,group,fillertreatment)

FillermaterialclassificationscanbefoundinCSAStandardW48“FillermetalsandAlliedMaterialsforMetalArcWelding”orAWSSpecifications:

Checkthelabelonthefillermaterialboxorspooltoobtainthefullfillermaterialclassification.Thisinformationcanalsobeverifiedonourwebsitewww.cwbgroup.org.

PleasenotethereisanewdesignationsystemforwireelectrodesanddepositsforGMAWofnonalloyandfinegrainedsteelsasspecifiedinISOCAN/CSA-ISO14341.

FulldetailscanbefoundinCSAStandardW48.

Page 18: CWB Welding Procedure Guide

Page 14 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

ThecommonlyusedclassificationsareB-G49A2CG3(formerlyER49S-3)andB-G49A3CG6(formerlyER49S-G).

Theelectrodeorelectrode-fluxcombinationforbuttjointsusingcompletejointpenetrationgrooveweldsshallbeinaccordancewithTable11.1or12.1ofCSAStandard.

Theelectrodeorelectrode-fluxcombinationfor:

completejointpenetrationgrooveweldsinjointsotherthanbuttjoints;•

partialjointpenetrationgroovewelds;or•

filletweldsmaybeoflowerorhigherstrengththanrequiredbyTable11.1or12.1,providedthatthe•conditionsofTable11.2(a),11.2(b),12.2(a),or12.2(b),asapplicable,arefullysatisfied.

RememberthatonlysteelsinColumn2ofTable5-3ofCSAStandardmaybeweldedwithSMAWwithotherthanlowhydrogenelectrodesandFCAWandMCAWwithoutdiffusiblehydrogendesignators.

Thefollowingfillermaterialgroupsmaybeusedforshieldedmetalarcwelding(SMAW):

Group ElectrodeClassifications

F1 EXX22,EXX24,EXX27,EXX28

F2 EXX12,EXX13,EXX14

F3 EXX10,EXX11

F4 EXX15,EXX16,EXX18,EXX48

Fillermaterialtreatmentshallbeinaccordancewithmanufacturer’srecommendationsandtherequirementsof the applicable standard.

SomecommonmistakeswithBlock6:

Thebasematerialisnotfullydescribed.Forexample:3XXStainlessSteel.Aprecisedescriptionmust•begivenfromthereferencecodesuchasGroupAorB,Table3.1,AWSD1.6.Aprecisematerialspecificationsuchas“ASTMA240,Grade304L”canalsobegiven.

Thefillermaterialclassificationisincorrect.•

Nothicknessisspecified.•

Page 19: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 15© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

4.7 BLOCK7(Weldingdetails)

Thickness

Recordthethicknessofmaterialtobeweldedinthespaceprovided.

Weldsize/ETT

Theweldsizeforafilletweldoreffectivethroatforagrooveweldshouldbeenteredinthissection.

Layerandpassnumber

Enterthenumberofpassesandsequenceofwelding.ThereareseveralwaysavailabletodeterminethenumberoflayersandpassesforaWPDSincluding:

• TheNomographMethod

• TheMathematicalEquationMethod

• TheWeldCalculatorProgramMethod

Thesemethodsrequireyoutocalculatetheareaofweldandtoselectadepositionrate.Depositionratescanbefoundinsomeweldingtextbooks,onlineorfromyourelectrodesupplier.

Steelandaluminumcalculators,Weld_ITsoftware,datasheetpreparationcoursesetc.areavailablefromthe CWB to help you calculate the number of layers and passes. Details can be obtained from our website www.cwbgroup.org.

Welding Processes

Enterthenumber“1”or“2”identifiedinBlock2ortheletterdesignationbelow.

Welding Process Letter Designation

ShieldedMetalArcWelding SMAW GasMetalArcWelding GMAW FluxCoredArcWelding FCAW MetalCoredArcWelding MCAW GasTungstenArcWelding GTAW Submerged Arc Welding SAW Plasma Arc Welding PAW Electroslag Welding ESW Electrogas Welding EGW Stud Welding SW

Page 20: CWB Welding Procedure Guide

Page 16 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

Diameter

ThestandardunitsofmeasurementforelectrodediameteraremminSI(metric)andinch(imperial).ThefollowingshowscommonelectrodesizesinSI(metric)andImperialunits.

INCH MM 0.030 0.8

0.035 0.9

0.040 1.0

0.045 1.2

1/16 1.6

5/64 2.0

3/32 2.4

1/8 3.2

5/32 4.0

3/16 5.0

1/4 6.0

Be consistent with the selection of the choice of units.

Wirefeedspeed

Thestandardunitsofmeasurementforwirefeedspeedarem/mininS.I.(metric)andinches/min(imperial).

A calibrated wire feed meter is preferred for measuring wire feed speed when the actual welding is in progress.Ifaverificationoftherecordednumberisnecessaryorawirefeedmeterisnotavailable,measurethelengthofwiredischargedfromthegunforaperiodof20seconds.Multiplythelengthofdischargedwireby3togivethewirefeedspeedininches/minuteormeters/minute.Takecaretoensurethat these are the real wire feed speeds and not the run in values

Current

Currentvaluescanbefoundinweldingtextbooks,onlineorbycontactingyourelectrodesupplierforoneoftheirproductcatalogs.Thecurrenttobeuseddependsonmanyfactorsincludingelectrodetype,size,weldingposition,jointdesign.

Measuretheamperageusingacalibratedclamptypeampmeter.Followthemetermanufacturer’sdirectionsandmeasuretheamperageasclosetothegun/holderaspossiblewithoutinterferingwiththeoperator.Thisusuallyisabout3or4feetfromthegun/holder.Whenmeasuringvoltagedifferenttechniquescan be used depending on the welding process being used.

Page 21: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 17© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

Voltage

Whenmeasuringvoltage,differenttechniquescanbeuseddependingontheweldingprocessbeingused.FortheSMAWandGMAWprocessesthevoltagecanbetakenbetweenthecableterminalsontheweldingmachine.

FortheGMAWandFCAWprocesses,thevoltagecanbetakenbetweentheworkleadattheworkconnectionclampandtheelectrodeleadatthethecontractorinthewirefeedunit.Ifnotpractical,thevoltagecanalsobetakenbetweenterminalorbetweenthecableterminalsontheweldingmachine.

FortheSAWprocess,thevoltagecanbetakenbetweentheelectrodeleadconnectionatthetorchandtheworkleadclamp.

Warning-Weldingparametersshouldonlybemeasuredbyproperlytrainedpersonnelfollowingsafeworkpractices.Followmanufacturersrecommendations.

Current Polarity

Enterthecurrentandpolarityfortheelectrode,electrode-gasorelectrode-fluxcombinationbeingused.Thisinformationcanbefoundinweldingtextbooks(CWBLearningCentreModule4),electrodestandards,online or from electrode catalogues or from your supplier.

Directcurrentelectrodepositive(DCEP)isthearrangementofdirectcurrentweldingleadsinwhichtheelectrodeisthepositivepoleandtheworkpieceisthenegativepoleoftheweldingarc.Anonstandardterm for this is direct current reverse polarity.

Directcurrentelectrodenegative(DCEN)isthearrangementofdirectcurrentweldingleadsinwhichtheelectrodeisthenegativepoleandtheworkpieceisthepositivepoleoftheweldingarc.Anonstandardterm for this is direct current straight polarity.

Alternatingcurrentisthecurrentflowinanelectricalcircuit,usuallyatapre-determinedfrequency.

ArcTravelSpeed/WeldingSpeed

Thearctravelspeedcanbemeasuredbyrecordingthetimetakentoweldaspecificlengthofweld,thenconvertthemeasuredtimeandlengthtoinches/minuteormillimeters/minute.Recordthecalculatedarctravelspeed(ATS)valueandnotjustthemeasuredlengthandtime.Thiscanbedoneusingoneofthefollowingformulas:

ATS(ins/min)= MeasuredWeldLengthininchesx60 MeasuredTimeinSeconds

orATS(mm/min)= MeasuredWeldLengthinmillimetersx60 MeasuredTimeinSeconds

Page 22: CWB Welding Procedure Guide

Page 18 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

Burn-offrate

Theburnofformeltingrateistheweightorlengthofelectrode,wire,rod,powdermeltedinaunitoftime.Record this information for arc spot welds.

Gasflowrate

Theshieldinggasflowrateshouldbehighenoughtomaintainadequateshieldingforthearcbutnotsohighthatitcausesturbulenceintheweldpool.Thegasflowratetobeuseddependsonanumberoffactorssuchastheprocess,weldingposition,shieldinggas,electrodeextensionandoperatingparameters.WithGTAW,flowratesaretypicallyintherangeof15to20cubicfeetperhour(CFH).WithGMAWandFCAWflowratestypicallyvarybetween25and45CFHdependingonthefactorsnotedabove.Manufacturer’sliteratureshouldbeconsultedformoredetails.

Thestandardunitsofmeasurementforgasflowratearel/mininS.I.(metric)andcubicfeet/hrCFH(imperial).ToconvertfromCFHtoL/minmultiplyby0.472.ToconvertfromL/minmultiplyby2.119.

CFH 15 20 25 30 35 40 45

L/min. 7 9.5 12 14 16.5 19 21

Checkthegasflowratewithameterandrecordtherateandtheunitofmeasurement(inbrackets).

Heat input

Entertheheatinputandtheunitofmeasurementwhentheheatinputneedstobecontrolled.Examplesarewhenweldingquenchedandtemperedsteelsandwhenspecificimpactpropertiesneedtobeachieved.

Heatinputistheenergysuppliedbytheweldingarctotheworkpiece.Theheatinputiscalculatedusingthefollowingformula:

H= VxAx60

1000xT

where:

H=heatinput(kJ/inorkJ/mm)

V=arcvoltage(volts)

A=current(amps)

T=travelspeed(in/minormm/min)

Page 23: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 19© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

SomecommonmistakeswithBlock7:

Nowirefeedspeedwithasemi-automaticprocess.(Thisisoneadjustmentthewelderneedstomake)•

IncorrectvoltageorwirefeedspeedparametersforGMAWsprayarctransfer.Chartsshowing•parameters for spray transfer are available from the CWB

Incompleterangeoffilletweldsizes•

Incorrectnumberofweldingpassesinflare-bevelorflare-Vjoints.Ex:8weldingpassestogetan•8mm effective throat

Noflowrateentered•

Flowrateunitwritten“CFM”insteadof“CFH”•

4.8 BLOCK8(Finalremarks)

Heattreatment(preheat,interpasstemperatures,postweldheattreatment)

ForpreheatorinterpasstemperaturesrefertotheapplicabletableinthestandardsuchasTable5-3,CSAStandardW59.AlternativelyenterthevaluesinCentigradeorFahrenheit.Thisboxcannotbeleftemptyormarkedasambientornotapplicable(N/A).

If a post weld heat treatment is used the temperature and time should be recorded.

Additionalremarks

Anyadditionalremarksorrequirementsshouldbeaddedinthissection.Itcanalsobeusedfornotesifthereisinsufficientspaceinothersectionsoftheweldingproceduredatasheetform.Examplesaredetailsof pulsed welding or welding techniques such as stringer or weave beads.

Companyauthorization

Thedevelopedweldingproceduresneedtobeacceptedbytheresponsiblepersonnelatthecompanybefore submission to the CWB.

ForcompaniesinvolvedincertificationtoCSAStandardW47.1-Division1or2,theirweldingproceduresmust indicate the acceptance by the designated welding engineer. Engineers submitting welding procedurestotheCWBmust,attheiroption,sealand/orsigneachdocument.

Page 24: CWB Welding Procedure Guide

Page 20 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

ForcompaniesinvolvedincertificationtoCSAStandardW47.2-Division1,2.1or2.2,CSAStandardW186,theirweldingproceduresmustindicatetheacceptancebythedesignatedprofessionalengineerresponsible for welding procedures and practice. Engineers submitting welding procedures to the CWB must,attheiroption,sealand/orsigneachdocument.

ForcompaniesinvolvedincertificationtoCSAStandardW47.1-Division3orCSAStandardW47.2-Division3theirweldingproceduresmustindicatetheacceptancebyaqualifiedweldingsupervisor.Weldingsupervisors submitting welding procedures to the CWB must sign each document.

ForDivision3companies,whentheweldingsupervisorchangesthecompany’sapprovedweldingproceduresarestillconsideredvalid.Thecompanyisnotrequiredtosubmittheexistingweldingproceduresforre-approvalorprovideanacceptanceletter.Thenewweldingsupervisoristestedontheknowledgeandapplicationofthecompany’sweldingprocedures.

WhenacompanychangesitsstatusfromDivision3toDivision1,2(W47.1)or2.1or2.2(W47.2),orwhenanengineertakesovertheresponsibilitiesforpreviouslyapprovedweldingprocedures,theengineermay,athisorherdiscretion,useoneormoreofthefollowingoptions:

prepareandsubmitforapprovalnewweldingproceduresbearinghisorhersealand/orsignature;•

issue a dated and signed letter to the CWB listing all welding procedures previously approved by the •CWB that have been reviewed and found to be acceptable for the company’s operations.

review,signand/orsealtheexistingdocumentsandresubmittheappropriatenumberofcopiesforre-•approval. If the welding supervisor’s or engineer’s signature or the engineer’s seal has been removed from the document then the previous approval must also be removed. If the previous approval stamp has not been removed the documents are returned to the engineer without being reviewed.

iftheengineerdoesnotsubmitanydocumentationtotheBureauregardingtheexistingprocedures,•it is presumed that the engineer has reviewed the procedures and found them to be suitable for the company’sweldingoperations.TheengineerisnotrequiredtoadvisetheBureauoftheactionheorshehastaken.

WhenacompanychangesitsstatusfromDivision1or2toDivision3,thecompany’sexistingapprovedweldingproceduresarestillconsideredvalid.Thecompanymaysubmittheexistingweldingproceduresforre-approvalorprovideanacceptanceletter,althoughthisisnotarequirement.

Date

Thedatasheetshouldhaveanaccepteddate.

SomecommonmistakeswithBlock8:

Weldingproceduredatasheetsarenotacceptedbytheauthorizedpersonnel.•

Preheatisenteredas“none”orambient.•

IncorrectPreheatisspecified.•

Page 25: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 21© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

4.8 CHECKLIST:Thefollowingchecklistcanbeusedforcompletingweldingproceduredatasheets.

+ If heat input control is required

WELDINGPROCEDUREDATASHEETITEM SMAW GMAW FCAW MCAW GTAW SAW

GeneralInformation

Company name and address X X X X X X

WPDS No. X X X X X X

Date and Rev X X X X X X

ProcessInformation

Reference Standards X X X X X X

Welding Process X X X X X X

Pulsed current X X X X

Shielding gas type X X X X

JointInformation

Positions X X X X X X

Process mode X X X X X X

Jointtype X X X X X X

Penetration X X X X X X

Fillet X X X X X X

Backingmaterialandthickness X X X X X X

Backgouging X X X X X X

Technicalinformation

Electrodeextension X X X X

Fluxclassification X

Tungstenelectrode X

Cleaning X X X X X X

Jointpreparation

Jointconfiguration/jointtype X X X X X X

Baseandfillermaterial

Identificationtostandardorgroup X X X X X X

Identificationoffillermaterial X X X X X X

Welding details

Thickness X X X X X X

Weldsize X X X X X X

Layers X X X X X X

Pass No. X X X X X X

Welding Process X X X X X X

Diameter X X X X X X

Wire feed speed X X X X

Voltage + X X X + X

Current,CurrentType/polarity X X X X X X

Arc travel speed + X X X + X

Gasflowrate X X X X X

Additionalitems

Heattreatment/preheat/interpass X X X X X X

Additionalremarks

Companyauthorization X X X X X X

Charpy V-notch

Reference standard X X X X X X

Heatinput X X X X X X

Stringer or weave bead X X X X X X

ArcSpotwelds

Visible diameter X X

Coatingthickness X X

Page 26: CWB Welding Procedure Guide

Page 22 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

5.0 SubmissionOfWeldingProcedures

AcertifiedcompanyisrequiredbytheStandardtosubmitweldingproceduredatasheets,totheCWB,forthe types of welded joints used by the company.

Electronic submissions of welding procedures should be sent to [email protected].

HardcopysubmissionsshouldbesenttotheProceduresDepartment,7250WestCreditAve.,Mississauga,ON L5N 5N1.

AWPDScanbeacceptedbasedonthefollowing:

• Thejointgeometryandparametersarespecifiedbythegoverningstandardtobeprequalified

• ThecompanyhaspreviousprocedurequalificationtestdatarecordedonaPQR(procedurequalificationrecord)

• TherearesuccessfulproceduredatasheettestsintheCWBdatabasethatmatchtheinformationonyour WPDS

• Bysuccessfullypassingprocedurequalificationtestsconductedinaccordancewiththerequirementsof the applicable standard

• Bysuccessfullypassingprocedurequalificationtestsconductedinaccordancewithotherrecognizedspecificationsorstandards

• BysuccessfullypassingaspecialprocedurequalificationtestrecordedonaPQR(analternativetypetest)

TherequirementsforprocedurequalificationtestingwillbeidentifiedbytheProcedureEngineerinalettersent to the client.

Page 27: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 23© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

6.0 ReviewAndApprovalOfWeldingProcedures

General

Each submission is reviewed by a Procedure Engineer based on the requirements of the applicable standardsand/orcodes.Theapplicablestandardand/orcodemustbereferredonthedocumentsubmitted.

TheProcedureEngineersusetheirprofessionaldiscretionwhenreviewingalldocumentstoensurethattheyarefeasibleandmeettherequirementsassetoutinthecertificationstandards.

WhenaWeldingProcedureDataSheetmeetsallprequalifiedrequirementsbutdoesnotseemfeasiblesoundness tests are required.

Incasesnotdirectlycoveredbythecertificationstandards,theProcedureEngineersapplythegeneralconcepts of the standard combined with the requirements of other relevant standards and codes to complete the review and approval process.

Welding Engineering Standards

Welding Engineering Standards when required are stamped received.

WeldingProcedureSpecifications

Weldingprocedurespecificationsthatsatisfytherequirementsspecifiedintheapplicablestandardarestamped accepted.

Weldingprocedurespecificationssubmittedforapprovalshallinclude,asaminimum,theapplicableessential variables of the governing design or manufacturing standard.

Welding Procedure Data Sheets

PrequalifiedJoints:Weldingproceduredatasheets,usingjointsdesignatedasprequalifiedinthegoverningstandard,canbeacceptedbytheCWBasprequalifiedwithoutfurthertestingbythecompany,providedallotherrequirementsofthegoverningstandardhavebeenmet.ExamplesofgoverningstandardsthatdesignatejointsasprequalifiedareCSAStandardW59andAWSCodeD1.1.

Page 28: CWB Welding Procedure Guide

Page 24 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

ApprovalusingtheCWBdatabase:WeldingproceduredatasheetsthatarenotprequalifiedinthegoverningstandardcanbeacceptedbytheCWBifsufficientrelevanttestinginformationhasbeenaccumulatedbytheCWB.TheCWBreviewsallsubmittedWeldingProcedureDataSheetsthatarenotprequalifiedagainsttheinformationinourdatabase.Thisdatabasecontainsprocedurequalificationtestscompletedbycompanies,andifsufficientinformationisfound,acceptancecanbegrantedwithoutprocedure testing. Welding Procedure Data Sheets that satisfy these requirements are stamped accepted on the basis of previous tests accumulated by the CWB.

NonPrequalifiedJoints-ProcedureTesting:WeldingproceduredatasheetsthatarenotprequalifiedinthegoverningstandardcanbeacceptedbytheBureauifrelevantprocedurequalificationtestingiscompletedbythecompanyandwitnessedbytheCWB.TherequirementsforprocedurequalificationtestingareidentifiedbytheProcedureEngineerinalettersenttotheclient.Weldingproceduredatasheetsthat are successfully tested are stamped accepted to the applicable standard on the basis of procedure qualification.

Morethanonequalificationstandard/codespecifiedontheWeldingProcedureDataSheet: If thereismorethanonestandard/code,therequirementsofallspecifiedstandards/codesmustbemet.Forexample:AfilletweldWeldingProcedureDataSheetwithbothCSAW47.1andAWSD1.6,willrequired3macro-etch tests.

Page 29: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 25© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

7.0 SampleWeldingProcedureDataSheetsCWB Form 160E/99-1

WELDING PROCEDURE WPDS NO.:DATA SHEET DATE: Rev.: 0

Company Name: Ref. Standards:

Address: Ref. WPS:

Welding Processes: Pulsed: Pulsed:Shielding Gas Type:

ETT=Material: Thickness:

Method:Depth:

Type: Dia.:

Part

III

Group

F4

Thick-ness (

)

WeldSize/ETT

PassNumber

WeldingProcess

Dia.( mm )

CurrentA

VoltV

CurrentPolarity

WeldingSpeed( )

Burn-OffRate

( )

Gas Flow Rate

( )

5.0 1 SMAW 3.2 120-140 AC/DC+ N/A6.0 1 SMAW 3.2 120-140 AC/DC+ N/A8.0 1-3 SMAW 3.2 120-140 AC/DC+ N/A10.0 1-4 SMAW 4.0 160-180 AC/DC+ N/A12.0 1-6 SMAW 4.0 160-180 AC/DC+ N/A16.0 1-7 SMAW 4.0 160-180 AC/DC+ N/A

Date:

To be signed by the engineer or supervisor before

submission to the CWB

Remarks: Preheat in accordance with Table 5-3 of CSA W59

5/27/2008

Interpasstemp.max.:Preheat min: 10° CInterpasstemp.min.: 10° C

Heat treatment : CWB Acceptance Company Authorization

1-3 N/A1-3 N/A

1-2 N/A1-2 N/A

1 N/A1 N/A

Heat Input( )

Joint Configuration & Pass/Layer Sequence

Special RequirementsIdentification of Base Material (for CSA W186 indicate carbon equivalent, max. phosphorus & sulphur content)

Tungsten Electrode:

LayerWire Feed Speed

( )

Nozzle Diameter(s):

SMAW-2F-85/27/2008

CSA W47.1/ W59Canadian Welding Bureau

N/A

7250 West Credit Avenue, Mississauga, ON L5N 5N1 SMAW-1

1 2N/ASMAW

Positions:Process Mode:Joint Type:

Horizontal

Use a chipping hammer and wire brush. Slag shall be removed from all finished welds and before welding over previously deposited metal.

CSA W186 Rebar Splice Type:

N/A

Penetration:

Flux Classification: N/A

Backing:

N/A

N/A

Electrode Extension:

Backgouging:

N/ACleaning Procedures

Identification of Filler MaterialSteels in Groups 1, 2 and 3 of Table 11-1/ 12-1

Thickness or Dia.

5.0 mm - 16.0 mm5.0 mm - 16.0 mm

Specification & Grade

Steels in Groups 1, 2 and 3 of Table 11-1/ 12-1

Process Trade Name Classification Filler Treatment

Welding Parameters

SMAW E4918 Cl. 5.2.2.4, W59

Yes No Yes No

Manual Semi-Auto Machine Auto

Butt Tee Corner Lap Edge

Complete Partial Fillet

Yes

No

Direct Splice Indirect SpliceRebar to Structural Member Only

Lap Splice

GAP 0-1 mm

231 4

567

SAMPLE

Page 30: CWB Welding Procedure Guide

Page 26 © Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

© Copyright CWB Group - Industry Services

CWB Form 160E/99-1

WELDING PROCEDURE WPDS NO.:DATA SHEET DATE: Rev.: 0

Company Name: Ref. Standards:

Address: Ref. WPS:

Welding Processes: Pulsed: Pulsed:Shielding Gas Type:

ETT=Material: Thickness:

Method:Depth:

Type: Dia.:

Part

III

Group

N/A

Thick-ness (

)

Weld Size/ ETT

PassNumber

Welding Process

Dia. ( mm )

Current A

Volt V

Current Polarity

Welding Speed

( mm/min )

Burn-Off Rate

( )

Gas Flow Rate

( l/min )6 1 GMAW 1.2 260 28 DC+ 400-500 20

8 1 GMAW 1.2 260 28 DC+ 300-400 20

10 1 GMAW 1.2 260 28 DC+ 400-500 202-3 GMAW 1.2 260 28 DC+ 400-500 20

Date:

To be signed by the engineer or supervisor before

submission to the CWB

In accordance with Table 5-3, CSA Standard W59

5/27/2008

Interpasstemp.max.: 250° CPreheat min: 10° CInterpasstemp.min.: 10° C

Heat treatment : CWB Acceptance Company Authorization

1 10.02 10.0

1 10.0

1 10.0

Heat Input( )

Joint Configuration & Pass/Layer Sequence

Special Requirements

N/A

Identification of Base Material (for CSA W186 indicate carbon equivalent, max. phosphorus & sulphur content)

Tungsten Electrode:

LayerWire Feed Speed

( m/min )

Nozzle Diameter(s):

GMAW-2F5/27/2008

CSA W47.1/ W59Canadian Welding Bureau

N/A

7250 West Credit Avenue, Mississauga, ON L5N 5N1 GMAW-1

1 290%Ar/ 10% CO2GMAW

Positions:Process Mode:Joint Type:

Horizontal

Wire brush, clean between passes

CSA W186 Rebar Splice Type:

16 mm

Penetration:

Flux Classification: N/A

Backing:

20 mmElectrode Extension:

Backgouging:

N/A

N/ACleaning Procedures

Identification of Filler MaterialASTM A36, A516 Gr. 70 G40.21Gr. 300W, 350 W

Thickness or Dia.

6-10 mm6-10 mm

Specification & Grade

ASTM A36, A516 Gr. 70 G40.21Gr. 300W, 350 W

Process Trade Name Classification Filler Treatment

Welding Parameters

GMAW N/A B-G 49A 3 C G6 (ER49S-6) Cl. 5.2.4.5, CSA W59

Yes No Yes No

Manual Semi-Auto Machine Auto

Butt Tee Corner Lap Edge

Complete Partial Fillet

Yes

No

Direct Splice Indirect SpliceRebar to Structural Member Only

Lap Splice

231

GAP 0-1 mm

SAMPLE

Page 31: CWB Welding Procedure Guide

© Copyright CWB Group - Industry Services Page 27© Copyright CWB Group - Industry Services© Copyright CWB Group - Industry Services

WELDINGPROCEDUREPREPARATION®

NOTES