Page 1: Transgranular Stress Corrosion Cracking

Transgranular Stress

Corrosion CrackingMUHAMMAD ARIF SAADILAH

1406507285

Page 2: Transgranular Stress Corrosion Cracking

Layout

Definition

Characteristics

Factors

Corrosion

Crack

Mechanism

Study Case 1

Page 3: Transgranular Stress Corrosion Cracking

Definition

Page 4: Transgranular Stress Corrosion Cracking

Factors Specific Crystal Planes

Low Indices: [100], [110], [210]

Speciffic Electrochemical

Page 5: Transgranular Stress Corrosion Cracking

Cracking Mechanism

Page 6: Transgranular Stress Corrosion Cracking

Characteristics of SCC

Page 7: Transgranular Stress Corrosion Cracking

Corrosion type: Pitting

Page 8: Transgranular Stress Corrosion Cracking

Prevention

Lowering the stress

Eliminating the critical environmental species

Adding Inhibitors

Coatings

Changing the material

Shot-peening / Shot Blasting

Applying cathodic protection

Page 9: Transgranular Stress Corrosion Cracking

Study Case

Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineriesAlmubarak and M. Belkharchouche & A. Husain

Anti-Corrosion Methods and Materials

Volume 57 · Number 2 · 2010 · 58–64

Page 10: Transgranular Stress Corrosion Cracking

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineries – Introduction -

Austenite

- H2S

- Sour Gas

- Polythionic Acid

Kuwait

Petroleum Reinaries

Page 11: Transgranular Stress Corrosion Cracking

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineries

– Materials-

• Annealed by 1080 C, thn

water quenching

• Sensitizing heat 650 C then

air cooling

Page 12: Transgranular Stress Corrosion Cracking

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineries – Methods-

Page 13: Transgranular Stress Corrosion Cracking

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait petroleum refineries

– Results-

Page 14: Transgranular Stress Corrosion Cracking

• Sensitized austenitic stainless steel type 304 in polythionic acid

• sensitized austenitic stainless steel type 304 in sour

solution

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineries – Results-

Page 15: Transgranular Stress Corrosion Cracking

sensitized austenitic stainless steel type 304 in chloride solution

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineries – Results-

Page 16: Transgranular Stress Corrosion Cracking

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineries – Results-

a) Sensitized austenitic stainless steel type 321 in polythionic acid;

b) sensitized austenitic stainless steel type 321 in sour solution;

c) sensitized austenitic stainless steel type 321 in chloride solution;

Page 17: Transgranular Stress Corrosion Cracking

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineries – Results-

Page 18: Transgranular Stress Corrosion Cracking

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineries – Result-

Page 19: Transgranular Stress Corrosion Cracking

the polythionic acid is the primary contributory agent for cracking

Types 304 and 316 stainless steel are unsuitable for longterm

exposure in sulfide service above 4008C because of sensitization.

sensitization evidently accelerates SCC and causes cracking to

occur easily

The present investigation was done in a short period (45 days)

for different grades of sensitized stainless steel where cracking and

severe SCC occurred.

Case Study: Stress corrosion cracking of sensitized

austenitic stainless steels in Kuwait

petroleum refineries – Conclusion-

Page 20: Transgranular Stress Corrosion Cracking

Terima Kasih