stress corrosion cracking of stainless steels in chlorides environments
TRANSCRIPT
![Page 1: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/1.jpg)
Stress Corrosion Cracking of Stainless Steels in Chlorides Environments
Joint EFC NACE WORKSHOP September 10, 2007 Freiburg, Germany
Thierry Cassagne
TOTAL E&P France
![Page 2: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/2.jpg)
2 -Joint EFC NACE Workshop, Freiburg 2007
Outline
What we want to avoidExamples of stress corrosion cracking field failures
InternalExternal
What is knownShort review on SCC of SS in chloride environments
What is unknownMissing or unclear answers
![Page 3: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/3.jpg)
3 -Joint EFC NACE Workshop, Freiburg 20073
What we want to avoid …
- Joint EFC NACE Workshop, Freiburg 2007
![Page 4: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/4.jpg)
4 -Joint EFC NACE Workshop, Freiburg 2007
Experience with internal SCC
22Cr duplex SS so far
Environmental conditionsHigh local chloride concentrationsHigh temperatures T>120°COxygen content close to nil
Residual stresses from welding or fabrication
Only a few cases of internal SCC
![Page 5: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/5.jpg)
5 -Joint EFC NACE Workshop, Freiburg 2007
Through wall internal SCC in 22Cr duplex
defect A defect A
![Page 6: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/6.jpg)
6 -Joint EFC NACE Workshop, Freiburg 2007
Internal SCC of duplex 22Cr heat exchanger tubes
transgranularSCC
Fracture surfaceExternal initiation (oil side)
![Page 7: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/7.jpg)
7 -Joint EFC NACE Workshop, Freiburg 2007
Experience with external SCC
Alloys involved have been:austenitic SS (304, 316L, 904L)22Cr duplex SS martensitic SS (17-4PH)
Environmental conditions
No coating or damaged coatingUnder insulation or notHigh local chloride concentrationsTemperature of RT for austenitic and martensitic SS, >100°C for 22Cr duplex
Residual stresses are usually from welding
Some cases of external SCC
![Page 8: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/8.jpg)
8 -Joint EFC NACE Workshop, Freiburg 2007
External SCC in 304 SS at welds
![Page 9: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/9.jpg)
9 -Joint EFC NACE Workshop, Freiburg 2007
External SCC of 22Cr duplex + sigma phase
Up to 20% sigma phase
![Page 10: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/10.jpg)
10
What is known …
- Joint EFC NACE Workshop, Freiburg 2007
![Page 11: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/11.jpg)
11 -Joint EFC NACE Workshop, Freiburg 2007
Influence of environmental parameters
Major environmental parameters influencing SCC:TemperatureChloride concentrationpHPotential (oxygen, oxidizing species …)
SCC occurs ≤ RT (very acid) or ≥ 50°C in neutral concentrated chloride environments
Pitting is necessary for SCC in neutral environments, not in acid environments
Oxygen may not be necessary in concentrated acidic chloride environments (ex. boiling MgCl2)
Acid ≠ neutral environments
![Page 12: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/12.jpg)
12 -Joint EFC NACE Workshop, Freiburg 2007
Influence of potential
SCC domains
Acid environments: SCC when passive film is unstable
Combrade CSC Bombannes 1990
10 N H2S04 + 0.1 M NaCl solution at RT
R. Staehle et al. 1979
![Page 13: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/13.jpg)
13 -Joint EFC NACE Workshop, Freiburg 2007
Influence of potential
304 SS 42%MgCl2
144°C
Necessity to be above a critical potential for SCC to occur in moderately acid and neutral chloride environments
Brauns W&K 1968
Sensitized 304 SS in 350 ppm Cl- water
Lin et al. 1981
![Page 14: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/14.jpg)
14 -Joint EFC NACE Workshop, Freiburg 2007
Influence of oxygen and chlorides
M. Speidel 1977
Cl- ppm
Oxy
gen
cont
ent p
pm
W. Huijbregts 1986
![Page 15: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/15.jpg)
15 -Joint EFC NACE Workshop, Freiburg 2007
Influence of temperature
cracking
no cracking
Tim
e to
failu
re (h
)
M. Speidel 1981
![Page 16: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/16.jpg)
16 -Joint EFC NACE Workshop, Freiburg 2007
Influence of pH
304 SS in NaCl
C: SCC, P: pitting, S: stains, O: no corrosion
J. Truman 1977
![Page 17: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/17.jpg)
17 -Joint EFC NACE Workshop, Freiburg 2007
Influence of mechanical parameters
The major parameters influencing SCC are:StressStrain rateCold work
![Page 18: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/18.jpg)
18 -Joint EFC NACE Workshop, Freiburg 2007
Stress
In 300 series austenitic stainless steels SCC occurs well below AYS
E. Denhard 1967
Boiling MgCl2 154°C 347 SS in boiling MgCl2 154°C
H. Spahn et al. 1973
![Page 19: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/19.jpg)
19 -Joint EFC NACE Workshop, Freiburg 2007
Stress Intensity
M. Speidel 1981 M. Speidel 1981
![Page 20: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/20.jpg)
20 -Joint EFC NACE Workshop, Freiburg 2007
Influence of metallurgical parameters
The major parameters influencing SCC are:Chemical compositionImpuritiesMicrostructure (austenitic, duplex …)
![Page 21: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/21.jpg)
21 -Joint EFC NACE Workshop, Freiburg 2007
Influence of composition
H. Copson 1959
Ni content %
Tim
e to
failu
re (h
)
U-bends in boiling MgCl2 154°C
cracking
no cracking
![Page 22: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/22.jpg)
22 -Joint EFC NACE Workshop, Freiburg 2007
Influence of composition
22% NaCl105°C
22% NaCl105°C
M. Speidel 1981 M. Speidel 1981
![Page 23: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/23.jpg)
23 -Joint EFC NACE Workshop, Freiburg 2007
Influence of structure
Comparison between austenitic-ferritic (duplex) and 300 series austenitic stainless steels in neutral aerated chloride environments
S. Bernhardsson 1991
![Page 24: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/24.jpg)
24 -Joint EFC NACE Workshop, Freiburg 200724
What is unknown …
- Joint EFC NACE Workshop, Freiburg 2007
![Page 25: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/25.jpg)
25 -Joint EFC NACE Workshop, Freiburg 2007
SCC of stainless steels is well understood for external crackingbut the temperature limit of the various grades is not so clear
There are very few data available concerning SCC in concentrated chloride environments with “low oxygen”
Internal SCC in concentrated production environmentsExternal SCC in concentrated chloride environments (drop evaporation)
The limits of use of the various SS in concentrated chloride environments are not precisely known
![Page 26: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/26.jpg)
26 -Joint EFC NACE Workshop, Freiburg 2007
Unresolved practical questions
Internal SCC
Can SCC occur in mildly acidic (pH 3-4) concentrated chloride environments in the absence of oxygen or low oxygen?
If so, what are the threshold conditions in terms of temperature, chloride concentration and oxygen level for the various stainless steel families
Results will depend on the nature of the salts (Ca2+, Na+, Mg2+) and salt mixtures
External SCC
What is the SCC resistance of SS when “degraded” by welding or else?
What are the temperature limits of higher grade austenitic SS? 904L, 6Mo …
![Page 27: Stress Corrosion Cracking of Stainless Steels in Chlorides Environments](https://reader031.vdocuments.site/reader031/viewer/2022012405/551e02ec4a79596b108b4995/html5/thumbnails/27.jpg)
27 -Joint EFC NACE Workshop, Freiburg 200727
Questions?
- Références, date, lieu