preparation of the bi 12 sio 20 thin films by the sol-gel method
DESCRIPTION
Preparation of the Bi 12 SiO 20 thin films by the sol-gel method. Š. Kunej , A. Veber and D. Suvorov Advanced Materials Jožef Stefan Institute. Outline. Introduction Aim of work Experimental Results Sapphire Si/SiO 2 /TiO 2 /Pt Spinel MgAl 2 O 4 Conclusions. - PowerPoint PPT PresentationTRANSCRIPT
![Page 1: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/1.jpg)
Preparation of the Bi12SiO20 thin films by the sol-gel method
Š. Kunej, A. Veber and D. Suvorov
Advanced MaterialsJožef Stefan Institute
![Page 2: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/2.jpg)
Outline
• Introduction• Aim of work• Experimental• Results
• Sapphire
• Si/SiO2/TiO2/Pt
• Spinel MgAl2O4
• Conclusions
![Page 3: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/3.jpg)
Introduction
SILLENITESILLENITE
MINITURIZATION
THIN FILMSTHIN FILMS
* M. Valant, D. Suvorov; J. Am. Ceram. Soc., 84[12], 2900-904, 2001
AgAg
“Bulk” Bi Bi1212SiOSiO2020*
(5.5GHz):
’ = 37.6
Qxf = 8100 GHz
f = -20 ppm/K
Tsint. = 850°C
Microwave technology
(LTCC)
![Page 4: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/4.jpg)
Aim of work
• Preparing Bi12SiO20 (BSO) thin films using sol-gel method
• Determining microstructure and thickness of BSO thin films deposited on substrates:– Sapphire
– Si/SiO2/TiO2/Pt
– Spinel MgAl2O4
![Page 5: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/5.jpg)
Experimental: SOL-GEL Synthesis
Used chemicals:Used chemicals:•Bismuth (III) nitrate
[Bi(NO3)3·5H2O]•Tetraethly orthosilicate
(TEOS) [Si(OC2H5)5]•Acetic acid
[CH3COOH]•Ethanolamine
[H2NCH2CH2OH]•2-ethoxyethanol
[C2H5OCH2CH2OH]
Vacuum drying
60°C/96h
Bi(NOBi(NO33
))
Acetic acid+
Ethanolamine
Bismuth Bismuth complex complex solutionsolution
SolSol
Bi(NOBi(NO33))33·5H·5H22
OO
Spin-Spin-coating coating (5000 rpm)
Firing:
300-700°C/1h
TEOSTEOS +2-
ethoxyethanol
Analytical methods:Analytical methods:
XRD XRD SEM SEM AFM AFMPyrolysis: 220°C/2min
4x4x
![Page 6: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/6.jpg)
Results
C / ( mol/l ) t / h
1.20 5
1.12 48
0.98 168
0.76 456
0.67 -
050
100150200250300350400450500
0,5 0,6 0,7 0,8 0,9 1 1,1 1,2 1,3
c ( mol/L )
time o
f gela
tion (
h )
Influence of solvent on gelation time :
![Page 7: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/7.jpg)
Results: SapphireResults: Sapphire
Spin-coating: 4 x 5000 rpm
Firing: 700°C/1h
![Page 8: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/8.jpg)
Results: Sapphire
d 400nm
![Page 9: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/9.jpg)
Results: Si/SiO2/TiO2/Pt
Spin-coating: 4 x 5000 rpm
Firing: 700°C/1h
![Page 10: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/10.jpg)
Results: Si/SiO2/TiO2/Pt
d 230nm
![Page 11: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/11.jpg)
Results: Spinel
Spin-coating: 4 x 5000 rpm
Firing: 700°C/1h
![Page 12: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/12.jpg)
Results: Spinel
d 300nm
![Page 13: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/13.jpg)
Conclusions• The Bi12SiO20 (BSO) thin films were successfully
prepared by the sol-gel method• The BSO thin film obtained on sapphire substrate is
porous with rough surface• Homogeneous BSO thin film of thickness 230nm was
obtained for the thin film deposited on Si/SiO2/TiO2/Pt substrate
• Thin film deposited on the spinel substrate shows homogeneous microstructure with grain size of 200-500nm.
Future work:• Optimization of BSO sol-gel precursor• Obtaining “denser” BSO thin films • Dielectric measurements of BSO thin films
![Page 14: Preparation of the Bi 12 SiO 20 thin films by the sol-gel method](https://reader031.vdocuments.site/reader031/viewer/2022020106/568136a8550346895d9e4cc1/html5/thumbnails/14.jpg)