oxidation of nickel- and cobalt-base … of nickel- and cobalt-base superalloys way 11 'hard...
TRANSCRIPT
![Page 1: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/1.jpg)
DMIC Report 214
March 1, 1965
OXIDATION OF NICKEL- AND COBALT-BASE
SUPERALLOYS
WAY 11
'HARD COPY $. -.ICROFIqIE $. (6-_"o
DEFENSE METALS INFORMATION CENTER
Battelle Memorial Institute
Columbus, Ohio 43201
ow
![Page 2: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/2.jpg)
The Defense Metals Information Center was established atBattelle Memorial Institute at the request of the Office of theDirector of Defense Research and Engin4ering to provide Govern-ment contractors and their suppliers technical assistance andinformation on titanium, beryllium, magnesium, aluminum, refrac-tory metals, high-strength alloys for high-tomperature service,corrosion- and oxidation-resistant coatings, and thermal-protec.tion systems. Its functions, under the direction of the Office ofthe Director of Defense Research and Engineering, are as follows:
1. To collect, store, and disseminate technical In-formation on the current status of research anddevelopment of the above materials.
Z. To supplement established Service activities inproviding technical advisory services to pro.ducers, melters, and fabricators of the abovematerials, and to designers and fabricators ofmilitary equipment containing those materials.
3. To assist the Government agencies andtheircon.tractors in developing technical data requirodforpreparation of specifications for the above ma-terials.
4. On assignment, to conduct surveys, or laboratoryresearch isveatigations, mainly of a short-rangenature, as required, to ascertain causes of trou-bles encountered by fabricators, or to fill minorgaps in established research programs.
Contract No. AF 33(615).lltProject No, 897S
Roger J. RunckDirector
SWR Ut01o in th" " re ort " "m. tr-mJAB •ne i MY b0 4 b een S xte ul, uotat
he o iriini tL autbor MD d th e ari n g ag em .
-tr Patent quest ioASLpear to be ..... . towa±e'arh is advised bttOre making u86 of the material. and where • cpy" ti.Z.h J m aVtJLerilB it E8,d . Fern OM .O b o t,,-further publioatior.,OIt Oo" tt t13PIES AVELILE RNM |.,
![Page 3: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/3.jpg)
CLEARINGHOUSE FOR FEDERAL SCIENTIFIC AND TECHNICAL INFORMATION, CFS'iINPUT SECTION 410.11
LIMTATIONS IN REPRODUCTION QUALITY OF TECHNICAL ABSTRACT BULLETINDOCUMENTS, DEFENSE DOCUMENTATION CENTER (ODOC)
I. AVAILABLE ONLY FOR REFERENCE USE AT DOC FIELD SERVICES.COPY IS NOT AVAILABLE FOR PUBLIC SALE.
r 2. AVAILABLE COPY WILL NOT PERMIT FULLY LEGIBLE REPRODUCTION.REPRODUCTION WILL BE MADE IF REQUESTED BY USERS OF 0DD.
0A. COPY IS AVAILABLE FOR PUBLIC SALE.
B. COPY IS NOT AVAILABLE FOR PUBLIC SALE.
Q 3. LIMITED NUMBER OF COPIES CONTAINING COLOR OTHER THAN BLACKAND WHITE ARE AVAILABLE UNTIL STOCK IS EXHAUSTED. REPRODUCTIONSWILL BE MADE IN BLACK AND WHITE ONLY.
TSL-121-2/14 DATE PROCESSED:
PROCESSOR:
III
![Page 4: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/4.jpg)
DMIC Report 214March 1, 1965
OXIDATION OF NICKEL-AND COBALT-BASESUPERALLOYS
by
C. H. Lund and H. J. Wagner
to
OFFICE OF THE DIRECTOR OF DEFENSERESEARCH AND ENGINEERING
DEFENSE METALS INFORMATION CENTERBattelle Memorial Institute
Columbus, Ohio 43201
![Page 5: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/5.jpg)
The new high-strength nickel-base alloys with chromiumcontents of about 10 percent do not have adequate oxidationresistance over their utef-l temperature range and requireprotective coatings.
Elements which promote oxidation resistance in super-alloys. are chromium, silicon, aluminum, and several ofthe rare earths, especially cerium.
Bor.on adversely affects oxidation resistance; so dotitAnium, molybdenum, and tungsten if over 0. 5 percent.
Oxidation can he beneficial if it produces a uniform ad-herent protective surface film, or if it produces a filmused to alter surface properties, such as to increaseemissivity.
TABLE OF CONTENTS
Page
SUMMARY .................................... .................... i
INTRODUCTION ......................................... ............. 1
FUNDAMENTALS OF THE OXIDATION OF Ni-Cr AND Co-Cr ALLO7S . ........ 1
GENERAL SURFACE OXIDATION....................... 3
Experimental Methods ...................................... ......... 4Oxidation of Superalloys.......................................... . . 4
INTERGRANULAR OXIDATION . ........................................... 16
Alloy Depl-tion Effects . . ............................................ 21
OTHER SUBSURFACE OXIDATION .......................................... 22
EFFECT OF STRESS ............................................. .... 23
REFERENCES ............ ...... .................................. 25
APPENDIX
ALLOY INDEX AND COMPOSITIONS . ....................................... A-I
![Page 6: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/6.jpg)
OXIDATION OF NICKEL- A14b COBALT-BASE SUPERALLOYS
by
C. H. Lund* and H. J. Wagner**
SUMMARY
The superalloys are oxidation resistant but all Intergranular oxidation is preceded by alloywill oxidize at high temperatures when oxygen is depletion ahead of the advancing oxide front. Thepresent. The rate of oxidation will depend upon compositional gradient that is produced can act asmany factors including alloy composition, tem- the driving force for continued metal-ion diffusion.perature, oxygen concentration, diffusion rates, The depleted zone also is weaker than the basicetc. Alloys designed for maximum strength will alloy, particularly in precipitation-hardenablenot have maximum oxidation resistance. There- nickel-base alloys where chromium, aluminum,fore, the application of superalloys is a corn- and titanium are preferentially oxidized because ofpromise between strength and oxidation consider- their relatively high affinity for oxygen. Loss ofations. When maximum strength and oxidation titanium and aluminum content is particularlyresistance are both desired, protective coatings detrimental to strength properties.are needed.
Unusual conditions of atmosphere or metal.Superalloys are very complex nickel- or surface can result in subsurface oxidation not
cobalt-base alloys containing closely controlled usually found in superalloys. For example, in-amounts of several elements. Each of these ele- ternal preferential oxidation of chromium ratherments can participate in the oxide formation dur- than nickel might occur in atmospheres that areing high-temperature exposure, their participation oxidizing to chromium and reducing to nickel, orbeing regulated by activation energy, diffusion, internal oxidation might take place under a sur-and heat of formation of the oxides, face that has been previously carburized. Pa-
rameters for internal oxidation are not clearly
General surface oxidation is the formation of defined.an oxide layer of relatively uniform thickness onthe surface of the alloy. Light surface oxidation Stress has an effect on the rate of oxidation.is often not objectionable and may even be bene- It appears that oxidation proceeds at a constantficial. Intergranular oxidation, on the other hand, rate with increasing stress until a "critical"can be a serious problem on thin sections or wire stress level is reached at which oxidation pro-when present in only small amounts. The pene- ceeds much more rapidly. Stress also producestration of the oxide front not only reduces the ef- spalling of even the tightly adherent oxides cffective cross section, but it can act as a notch to most superalloys when sufficient shear is pro-reduce fatigue resistance. It can also be very , duced at the metal-oxide interface to causeserious in notch-sensitive materials. Fortunately, cracking. Under these conditions oxidation isintergranular oxidation takes place only at rela- rapid as fresh metal is continuously being exposedtively high temperatures. Superalloys, particu- for further reaction.
larly the precipitation-hardenable nickel-basealloys, are susceptible to intergranular oxide
penetration.
*Chief Development Metallurgist, Martin MetalsCompany. Wheeling, Illinois.
*::.Fcrrous and High Alloy Metallurgy ResearchDiv s inon , flttlle Memorial Institute,
Columbus, Ohio.
![Page 7: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/7.jpg)
INTRODUCTION are highly susceptible to the formation of oxideskins and films during melting and casting.
All of the superalloys will oxidize at high Cobalt-base alloys on the other hand do not, as a
temperatures when oxygen is present in the envel- rule, depend upon the precipitation of anoping atmosphere. The rate of oxidation depends aluminum-titanium-bearing compound for theirupon alloy composition, temperature, oxygen con- strength and thus are not nearly as susceptible tocentration, oxides formed, diffusion rates of the oxide formation during melting and casting. Thus,metals in both base metal and oxide, diffusion vacuum melting and casting are considered bens-rate of oxygen in the oxide, solubility of oxygen in ficial for only a few of the cobalt-base superalloys.the matrix, and a Lost of other variables. Oxida-tion may produce a general, uniform surface FUNDAMENTALS OF THElayer, or it may occur as intergranular penetra- OXIDATION OF Ni-Crtion along the grain boundaries, as subsurface AND Co-Cr ALLOYSpreferential oxidation (so-called "internal oxida-tion"), or as all three combined. The superior oxidation resistance of nickel-
chromium alloys has been recognized for overThe effects of oxidation can be beneficial, or 50 years. Among the first to recognize this fact
they can be harmful to the extent of causing cata- was Marsh, whose 1906 patent describes the im-strophic failure. Examples of beneficial oxides portant contribution of chromium when added toare the black oxides deliberately formeA n" thle mckel. Nickel-chromium alloys containing aboutRen' 41* skin of Mercury space capsules and on 20 per cent chromium have been standard forthe Inconel X (presently designated Inconel alloy many years in applications where electrical resis-X-750) skin of X-15 research aircraft. These tance, particularly at high temperatures, is im-oxides are formed to increase the emissivity of portant. These alloys also served as the basis ofthe surface and thus help to dissipate the tremen- the first superalloys, when it was discovered thatdous amounts of heat generated on the metal sur- they could be made precipitation hardenable by thefaces during reentry and high-speed flight, addition of small amounts of titanium or alumi-Catastrophic failure from oxidation occurs in thin numn, or both. In recent years, there has been asheets and fine wires subjected to temperatures tendency, among those engaged in superalloy de-too high for even short-time exposure. Other velopment, to retain only a minimum of chro-examples are given later in this report. mium, an amount just sufficient to provide ade-
quate resistance to oxidation and sulfidation.In general, the oxidation resistance of the Whereas the early nickel-base superalloys con-
nickel- and cobalt-base alloys is considered to be tained 16-20 per cent chromiurn, the later onesrelatively good. The oxides formed are tightly contain 10-15 per cent, a portion of the chromiumadherent and protective. This is especially true being displaced by elements contributing more toof the simple solid-solution type of alloys up to strength but less to oxidation resistance. The in-temperatures in excess of 2000 F and of most fluence of chromium on the oxidation resistance ofother alloys at temperatures up to about 1850 F. nickel is shown in Figure l(l)* and Table 1(Z).Above this temperature, oxidation becomes aproblem in the more complex superalloys. Addi- Cobalt-base superalloys also contain a rela-tions of many of the elements that give the alloys tively high proportion of chromium, usually aboutelevated-temperature strength (e. X., titanium 20 to 25 per cent. One of the reasons for the useand molybdenum) decrease the oxidation resis- of chromium is shown in Figure 2, which illus-tance. Aluminum, too, when participating in the trates the oxidation rate as a function of chromiumformation of certain strengthening phases, such content( 3 ).as gamma prime, may promote decreased oxida-tion resistance even though it is generally a bene- Simple binary nickel-chromium alloys haveficial element when in solid solution, excellent oxidation resistance, provided sufficient
chromium is present. Thus, Figure I shows thatWe are concerned not only with the problem additions of up to 5 per cent chromium actually
of oxidation of nickel- and cobalt-base alloys decrease the oxidation resistance at all tempera-under service conditions, but also with the control tures up to 1200 C (2200 F) and that further addi-of oxidation during melting, the importance of tions of chromium are required to reverse thewhich is shown by the interest in recent years in trend and impart superior oxidation resistance.vacuum and protective atmosphere melting of Figure 1 also shows that some minimum amountnickel-base superalloys. Because nickel-base of chromium is necessary to insure good corrosion
alloys contain large amounts of such highly re- resistance at various temperatures, the amount
active elements as aluminum and titanium, they increasing from about 12 per cent at 900 C (1650F)to about 18 per cent at 1200 C (2200 F). Similar
*Compositions are given in the Appendix. data are given in Table 1, taken from work by
Throughout this report the trade names used arethe ones current at the time of the investigation. *References are given on page 25.
![Page 8: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/8.jpg)
320 TABLE 1. OXIDATION DATA FOR NICKEL-0 1CHROMIUM ALLOYS(M)30 - - 1200C'--
1096 C (2000 r)28 - 76 cm Hg of 02
260-
2 Wt% Ate (gSc-4owAlloy Cr Cr sac- ) - K05Ko
E %. 22 1 0.00 0.00 5.48x 10-10 1.00E 2 0.3Z 0.36 Z3.6x 10-10 4.30
1200 1100 C 3 0.92 1.04 29. 7x 10- 1 0 5.424 2.00 2.25 39.6x 10-10 7.2Z
I5 3.45 3.88 46.8 x 10-10 8.55- 6 5.67 6.37 58.5 X i0"10 10.7
4-IS 7 7. 64 8.55 6 7.8 x 10-10 12.4108 8.71 9.70 30.8x 1010 5.634 9 11.10 12._0 3.79x 10-10 0.69
2 10 14.90 16.50 0.35 x 10-10 0.064
20.0 22.0 0.07 0. 013(a)Co 100 (a) Given in private communication by Dr. -. A.
Gulbransen of The Westinghouse Research
0 .U,. V-,-Laboratory.
Xp=parabolic rate constant for alloy-I W Kpo a parabolic rate constant for nickel
X
0 2 4 6 8 10 12 14 16 18 20Chromium Content, per cent -4914 000 ointly
CoO $coleFIGURE 1. DEPENDEfNCE OF DEGREE OF Terminal valuesOXIDATION ON THE CHROMIUM CONTENT I00 Cr3 03 scaleOF BINARY NI-Cr ALLOYSM1 with dissolved NSpecimens held 8 hours at temperature. 0 do d
° __ _ _""
Zima(2 ), which shows that the oxidation rate in- .C, 0creases with increasing chromium content up to 0
about 7. 5 per cent chromium and then rapidly de- .u -creases between 7. 5 and 11. 1 per cent. Between 0 0 ,11. 1 and ZO. 0 per cent chromium, there is a 1. -
gradual decrease in oxidation rate with a mini-mum at ZO per cent. The behavior of the cobalt- 00
chromium system, shown by the curves in Fig- . nure 2, is similar to that of the nickel-. chromium- 0.1system.
The chemical nature of the oxide films formed ,on nickel-base and cobalt-base alloys containingchromium varies with temperature and withchromium content. Chromium oxide (Cr 2O3 ),nickel oxide (NAG), and cobalt oxide (CoO), are valuesthe stable oxides usually found in the oxide scales Crs 0, scoleof nickel-chromium and cobalt-chromium alloys. O.OOI -
The actual composition of the oxide layers changes g00with temperature and time. In certain alloys with Weight Per Cend Chromiumthe base composition 8ONi-2OCr, it has been re-ported that NiO is the first oxide to form at low FIGURE 2. FIRST PARABOLIC SCALINGtemperatures (approximately 750 to 930 F) after CONSTANT VERSUS ALLOY COMPOSITIONshort periods of time(4 , s,6), or at about 2150 F FOR Co-Cr ALLOYS HEATED IN AIR( 3 )
![Page 9: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/9.jpg)
3after long oxidation times and cyclic heating. (4) very protective. Aluminum is also important inBetween 930 F and 1300 F, Crz03 has been ob- oxides formed at lower temperatures. When alu-served to form. At higher temperatures around minum is present, a dense inner layer of A12 0 3
S1650-1750 F, complex double oxides are formed is formed. However, it does not always effec-called spinels. For nickel-base alloys, the spinel tively slow down the diffusion of metallic ionsis usually designated as NiO.Cr 2 O 3 or as through the metal-oxide interface to the outer sur-NiCrZO 4 . At high temperatures the oxides face, which would be necessary for improved pro-formed are in two layers, an inner layer of tection of the alloy. Hagel( 8 ) investigated a vari-CrzO3 adjacent to the metal, and an outer layer ety of iron-aluminum, iron-chromium-aluminum,of spinel. The thickness of the spinel layer in- nickel-aluminum, and cobalt-aluminum alloys atcreases with time and temperature. temperatures between 600 and 1350 C in low-
pressure oxygen. He reported that the defectSpinels also are of varying composition, the structure and metastability of "y-A12 0 3 are the
CrZ0 3 content increasing with increasing time and principal reasons for the ineffectiveness of alu-temperature. According to Ignatov( 5 , 6 ), nickel- minum in preventing oxidation of these alloys.chromium spinels begin to decompose at tempera- Below about 900 C, y-AI 2 0 3 is formed, whichtures between 1100 C (2010 F) and 1200 C (2190F) permits the passage of nickel, cobalt, and ironinto the components NiO and CrO. The decom- ions through the layer, becoming oxidized to NiO,position of the spinels has an important influence Co 3 0 4 , '.nd Fe 3 0 4 , respectivzly. The transfor-on the oxidation process because it permits CrO mation from y-AlZO3 to a-AlZOS occurs betweento be yaporized from the surface, increasing the 900 C and 1100 C, and is accompanied by volumedriving force for the diffusion of chromium changes which can cause fissuring of the scale.through the oxide scale. Increased diffusion of Above 1100 C the a-Al 2 0 3 is effective in protect-chromium ions results in more oxidation. (7) In ing iron. Some NiO and NiAlZO 4 may still form,nickel-base alloys,, the diffusion of nickel ions but cobalt is not protected. The beneficial effectthrough the scale is negligible so that oxidation of chromium is due to the extension of the a-Al 2 0 3rates are dependent upon the rate of chromium in solution with a-Cr 203 down to 600 C.diffusion. In cobalt-base alloys, the diffusion ofcobalt ions is faster than that of chromium ions Examples of elements that adversely affect
so that CoO is found in the outer oxide layers. the oxidation resistance of Ni-Cr alloys are boronGradual buildup of CrO in the oxide scale results (over 0. 1 per cent), titanium, molybdenum, andin an increasingly effective barrier against diffu- tungsten (the latter three when over 0. 5 persion of cobalt ions, and hence a slowing down of cent). (6)
the oxidation rate. (3) It is generally accepted thatthe composition of the oxide films is determined According to the Soviet investigators, addi-by the relative activation energies of diffusion of tions of cerium, thorium, and several of the rarethe alloy components and the heats of formation of earths improve the high-temperature oxidationthe various oxides. (7) The reaction usually resistance of the nickel-base superalloys byoccurs by diffusion of the metal ions through the alloying with the NiO-Cr 2 0 3 spinel and preventingscale rather than by inward diffusion by oxygen, the rapid vaporization of Cr203 at temperaturesHowever, Ignatov states that oxygen diffusion in- of about Z000 F and above.( 5)ward is observed at temperatures of about 1000 C
(1830 F) and up. (6) GENERAL SURFACE OXIDATION
Superalloys are very complex alloys contain- General surface oxidation can be defined asing closely controlled amounts of several ele- the formation of an oxide layer of relatively uni-
ments. Each of these elements can larticipate in form thickness on the surface of the alloy. Mostoxide formation during high-temperature expo- often, this type of oxidation is evaluated by mea-sure, their participation being regulated by ac- suring the weight change of a sample after ativation energy, diffusion, and heat of formation specified exposure time or continuously duringof the oxides, as previously mentioned, the test. A weight gain may be the result of oxy-
gen (and, sometimes, nitrogen) pick-up duringSome of the elements commonly present in oxidation, whereas a weight loss may be the resu1'
superalloys are considered to be beneficial to of spalling of the surface scale. When oxide scaleoxidation resistance, i. e. , they contribute to the is lost, the weight of the scr 1.e lost is the sum offormation of a stable oxide. Examples of these the oxygen plus the metal contributing to the oxideare silicon, aluminum, and several of the rare- formation.* Because metal that is spalled mustearth elements, especially cerium. Aluminum first be oxidized, it is possible for a metal or anplays the most important role. If aluminum is alloy, at any given time, to show no net weightpresent in amounts of about 3 per cent or more ch•.nge (if adherent oxide weight gain equals loss(depending upon temperature), a spinel NiO.AIZ0 3
(or NiAlZO 4 ) is formed, which is mutually solublewith NiO.CrZO 3 (NiCr z 0 4) at temperatures of Y*Intergranular oxidation or oxidation of a second
about 1300 to 1900 F.(9) These spinel films are phase may cause weight loss if grains are lost.
![Page 10: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/10.jpg)
4of metal in scale spalled), suggesting that the formed during exposure. These methods, ifalloy is inert to its surroundings. Naturally, this properly carried out, result in a more direct in-wouLd not be true. dication of the amount of metal lost as a result of
oxidation, than is indicated by weight-gain mnea-Experimental Methods surements. Accordingly, the data presented by
different investigators for various alloys must beThe above illustration serves to point up the carefully analyzed in terms of test procedure
need for great care in performing and in inter- used. In this report, experimental data obtainedpreting oxidation studies. Because of the many under essentially similar conditions have beenvaria:leii involved, it often is difficult to compare plotted on the same graphs in order to comparetest results unless they are run under identical results.conditions. Temperature, oxygen partial pres-sure, and specimen surface roughness are just a Oxidation of Superalloysfew of the possible variables. If the oxide layerspalls off, weight-gain data can be quite errone- Figures 3 and 4 show the oxidation resistanceous. Probably the most reliable experimental of the Nimonic family(9% 10) of alloys plus a fewmethod is to test the specimen in a refractory cup data points for Haynes Stellite Alloy 31. (11) Inso that cup and contents can be weighed at inter- these tests, the loss of metal by oxidation isvals. In this manner, any scale falling from the indicated by the weight loss. Each specimenspecimen will be retained and weighed, was descaled electrolytically in caustic soda
after exposure. Before descaling, these alloysSome investigators choose to use mechanical would have shown a weight gain. Figure 3 gives
or chemical methods for removing the oxide the results of oxidation during continuous
12 12H.S.31 A-9 BOA 8 -
II Cobalt BassM _ j1 R80A 1_____ 8-900B/-90 8-75 I
,o / I10 [-0I
,IA'95 IA-99 9 ig--,n
-A (Reference 10) 18 . (Reference 9 )- A . 8 -E -1eferees0 .-Numbers signify alloy designat- VB- 7 Numbers sencif alloy sn Ii
(Reerece) V 6 -N-nbersfp signif allo de7'"ions(Nimonics 75,80A,90,95, 8-105 I " natmns(Nimonics 75, IOA,100 aInd 105_)_ _ ,/I . 90,95,100,105)
- 6
V a 5
IL . 4
All.!l
7EAIN Soo FO 9FO00 1OURS 110 700 SETIG IXN 9I O 00 1000S 1100D;•
TO ROOM TEMPERATURE EVERY 24 HOURS •
Weigt loe deermied ater escaingWeight lose determined after descaling elec-Aelectrolytically in caustic soda. trolytically in caustic soda. S
![Page 11: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/11.jpg)
exposure to air for 100 hours at various tempera- (2) the marked increase in oxidation resistance
tures, whereas Figure 4 gives data for specimens imparted by aluminum. Nimonic Alloys 100 and
subjected to intermittent heating in air. For the 105 have about 5 per cent aluminum (also a lowlatter test, each specimen was cycled from the titanium content), whereas the other alloys have
¶ftest temperature to room temperature and back lower aluminum contents, 2 per cent or less
once every 24,hours. (9, 10) (also higher titanium contents). Tuimnarev andPanyushin(1 ) obtained similar results, as shown
Two items of importance are shown by these in Figures 5 and 6.data: these are (1) the excellent resistance to
oxidation of the nickel-base superalloys and Figure 7 gives data for two of the newernickel-base alloys, IN-100 and SMZ00. The datafor IN-100 and SM200 are reported as a weight
gain, indicating that the scale remained on the4 specimens. These data are for 2000 F.( 1 2 ) Al-
though lower temperature data are not available,it is expected that the alloys would show less dif-
4 ference in performance at temperatures under2000 F.
Figure 8(13) illustrates the behavior of cer-
56 t tain nickel-base alloys that were subjected to\ 320
11200 C32 300 - - 4% Cr
2. - 9% Cr
N I 3. -2 %Cr"E 2°\ -2---
26C 4. - 12% Cr
24F 1 5. -16 % Cr
-1 220* I\\ I1100IC E
.2 20 200
CLC
Ia 2I2 A'-
4 160
i i2
O0 2 4 6 8 I0l
Aluminum, per cent A-491320 2 4 6 8 0 12 14 16 18
Aluminum, per cent A-49133
FIGURE 5. OXIDATION RESISTANCE OF NICKELALLOYS CONTAINING 12 PER CENT CHROMIUM FIGURE 6. OXIDATION RESISTANCE OF ALLOYSAND VARIOUS AMOUNTS OF ALUMINUM( 1 ) CONTAINING VARIOUS AMOUNTS OF
CHROMIUM AND ALUMINUM( 1 )
Specimens held 8 hourq at temperature. Specimens held 8 hours at temperature.
![Page 12: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/12.jpg)
5 6 __ _"___ 6
N6
S30.1
0 20 40 60 1400 0 -
FIUE7.XIAINBHAIRO MZO______ __'aN 3 N-0 AT00 F00F(
S t9 ~-03 -.1 8o -2 0 ( no M n ) I
._m / -0.4-
.2 J(P ISM 200 0.4 '
ineritethetng t a asme ha f h
•,0.3-
0 20 40 60 80 100 ,Q.OxiotonTiehr A-491410.
theto oxide scleh Nimonic 75
FIGURE 7. OXIDATION BEHAVIOR OF SM200AND INrl100 AT 2.000 F(I Z) -
02 --
intermittent heating. It was assumed that if the Ospecimens showed a weight loss it was because allthe oxide scale had spalled off. The likelihood -0.21_
was discounted that simultaneous weight gain from |
oxidation and partial spalling would account forlow losses or gains in weight. For these experi- -0-6ments, an intermittent heating cycle consisted oýl
inserting a rack of test specimens for 15 minutes -0.8into a furnace held at the test temperature andthen removing the rack for 5 minutes. This cycle -1.0was repeated 3000 times, for a total e'apsed time 80. 0(withMn} 1800of 10G0 hours. -1.2
-1A1
Figure 9(14) shows some of the data from the 0 200 400 600 8M o000same work, comparing the resistance to spalling A-49145of several nickel-base and iron-base alloys. It Total Elapsed Ti-e, hrmust be borne in mind that the percentage loss in
TABLE Z. DEPTH OF OXIDE PENETRATION OF FIGURE 8. BEHAVIOR OF NICKEL ALLOYS
SOME ALLOYS AFTER 1000 HOURS DURING INTERMITTENT HEATING(1 3 )
OF CYCLIC EXPOSURE IN AIR AT Specimens inserted in furnace for 15 minutes,1800 F removed from furnace for 5 minutes. Total.
____elapsed time, 20 minutes per cycle. Speci-men size, 0. 031 in. x 3/4 in. ?: 3 in.
Penetration After
3000 Cycles toAlloy 1800 F (1000 hr.), in. weight due to spalling is always higher than is the
gain in weight observed when the scale is adher-
Nimonic 75 0.005 ent. This is because, in the first case, the lossis due to metal loss, but the weight gain is due to
Inconel (Pre-1951) 0.012 oxygen. Accordingly, it is instructive to look alsoat the depth of penetration, calculated from a corn-
AISI Type 330 Steel 0. 0050 parison of the original thickness with the thicknessof unattacked metal remaining after the test.
'ncoloy 0.0062 Table Z shows these data for the 1800 F exposure.It is clear from these data that Nimonic 75,
AISI Type 310 Steel 0.0052 Types 330, 310, 309, and Incoloy were nearlyalike in terms of penetration, a fact not evident
AISI Type 309 Steel 0. 0064 in Figure 9.
![Page 13: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/13.jpg)
7
Total oxidotlof10v rInforgv uwle or oRlallon
W200- - *off o-wo-ton
a 70n X 25W MP F MF MP MIP 257025MF 2540F
o o 42400.
j 2300-
.50 2100.
11000 -
1900.
Inca 702 Inconel hMconew wconeix C-a
Total Elop!d Ti, FIGURE 10. COMPARATIVE OXIDATION(15nmiol at WF,5mlncoin k) CHARACTERISTICS OF HIGH-
TEMPERATURE SHEET ALLOYS( 1 4 )
FIGURE 9. BEHAVIOR OF SEVERAL NICKEL- Cross-sectional loss in thickness after100-hour exposure to a slow-moving airINTERMITTENT HEATING(14) atmosphere. t, the thickness of the sheet,
was not given. The data are for com-See Figure 8 for details about test. parative purposes only.
Figure I0(14) shows the relative oxidation (a) This alloy was not identified in the
characteristics of several alloys after exposure paper. However, it can be assumed
to slow-moving air at various temperatures. No that it is L-605 (Haynes Alloy 25).
details of test procedure or sheet thickness were _ __
given in the source, so the data can be used forcomparison purposes only.
Scaling of Rene 41 sheet was reported byChilders and Simenz( 1 5 ) for temperatures between 06 -)1650 and 2000 F. Figure 11 summarizes the ef- U
fect of time and temperature on the scale thick-ress for 0. 010-inch-th'k sheet heated in air.
•0.4 10 Hus
Scaling and subscale reactions in Rene 41 0sheet and cast Udimet 700 were recently reportedby Wlodek( 1 6 ) for the temperature range 1600 F to I-2000 F. Figures 12 and 13 show the results forsolution- annealed material on a log-log plot, and 10.2 1 -- 0 0
indicate the change from linear to parabolic rates. 0 HourelFigures 14 and 15 show the linear portions on alinear plot, and also indicate that the rates for I Houraged material and annealed material may be dif- 0ferent. Subscale reactions are discussed later in b600 100 law 1900 2000the present report, under the section covering Temperature, Falloy depletion effects.
FIGURE 11. EFFECT OF TIME AND TEMPERA-Measurements of the charge in thickness of TURE ON SCALE THICKNESS IN 0.010 IN.
Rene 41 sheet specimens exposed for 50 hours to RENt 41 HEATED IN AIR( 1 5 )
![Page 14: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/14.jpg)
8
S10.0 10.
1 4 4' L
if- Solution annealed Auio noe
0a 0.01
Time, minutes A-40121 Time, minutes A-91
FIGURE 12. LOGARITHMIC PLOT OF SPECIFIC FIGURE 13. LOGARITHMIC PLOT OF SPECIFICWEIGHT GAIN AGAINST TIME FOR A SINGLE WEIGHT GAIN AGAINST TIME FOR A SINGLEHEAT OF RENf9 41 SHEET( 1 6 ) HEAT OF CAST UDIMET 700(16)
O3- R ne'-41 08 2 0
+--+ Agd0 0.7- - Udimet 700-~.'--Annealed .E 600mm~e
- -- --- ~r iii s*cKAnnlealed0 .2C
IF CI OOOIT 0.
0.1 ;
/ 00
-16
4..
Time 120 1640F 0 03 40 06070miu+ -S1 Time, minute £41
So0to 20 ee 30 W m So 150 F;o ge Souto 10nealed 40 h.250 F; Tgd4Or
4 hr, 1600 F. 1975 F+24 hr, 1550 F +16hr, 1600 F.
moving air indicate increases in the order of tures between 1600 and 2200 F are shown in Fig.-0. 2-0. 3 mile at 1200 F, 0. 2-00.6 mile at 1500 F0 ure 16. A linear rate curve (slope = 1)1is seenand 0. 9 to 1. 4 mils at 1800 F. (17) Average oxi- for initial oxidation at 1600 F (for over 2000 min-dation (scaling) per side would be half of these utes), but this is ultimately replaced by a para-values. bolic rate (slope a 1 /2). The same behavior
occurs at 1800 F, but the linear rate persists forWlodok~la) recently reported on the oxidation only 200 minutes. The results shown in Figure 16
of Hastelloy X sheet. Both scaling and subacale are for a single heat; a second heat showed goodreactions occurred; the latter are discussed later duplication of these results at 2000 and 2200 F,in this report. The results of continuous weight but had over 100% greater parabolic rate constantmeasuretments made on Hastelloy X at tempera- at 1800 F.
![Page 15: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/15.jpg)
10.0 9
1.00
Tim, mItT ''" 01
Oxiato oox thied nike 0D.4 PonosTD
forunoatd pe imensa, miumt rzdi i- Srietmeaues up to 215 Ft r0 reco
sEIHow Tosdrbyhge weigh gainNS atM 1800 FA attNckE aIGRE pr8e.e OInAIO FgRES1for200 FOHAnd Olghl lAess O at8 R 90 BANDA 2000 F, thnrpreYb xoue
di xicdltieson compahringd oxdaione (Da ota ' Som ineetnTat nteefto aiuNickl) as oudid byNAS(19) an thereslts celemet on trohue oxidaion e reyithne pofuc a 0co 0)
Oxida. Ntio resisttne ofiato TrWt 1900 aenew 41 exniel-obl based onoialloy wraes pWoided byiicrueepreistnt pigrecision cating N Alloykr, ded-utinminain s whic he basey aluniorm w scaling
60w osdrbyhge egtgi t10 F tak r rsne nFgr 8fr20
an 4lgtyls8 a 00F hnrpotdb xoue
Wldka ) hssre oilsrt h eeadfiutes ncmaigoiaindt.Sm neetn aao h feto aiu
elmnso h xdtonrssac facm
31 ~ ~ ~ ~ ~ ~ ~ ~ ~ ~ ~ ,0 2,6F(uot _____ __________
Cr
Time, oursShoot5
FIGURE 17. LIEA PLTOFPCFCWIH ANAANS IEFRTOITDNCE(
![Page 16: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/16.jpg)
10
12 lese it a111 oftp We#. is not
0A. "T N42661 SIM4m. +10 50
Will 628+2,4 il o SO 910 -.
010*0@ it 498, wf U1 &
01106 34145*liee v I a300eKoKg-02u~c et s 3"W lo
X WN AIW-- I-
zeroTempm'Mure. C
0 FIGURE 20. COMPARISON OF TEMPERATUREgoo90 100 10 EFFECT BETWEEN K42B TYPE ALLOYS
Temperature, C A-4912. MODIFIED WITH MOLYBDENUM ANDWITH TUNGSTEN( 2 1)
FIGURE 19. EFFECT OF TEMPERATURE ON Total weight loss after 400 hours treatmentK42B AND MODIFICATIONS WITH STAINLESS recorded. Specimen size constant, .5/32 inch18-8 AND NICHROME FOR COMPARISON( 2 1) x 7/8 inch x 3 inches.
The data indicate total loss in weight after 400 0.0 --4 ~-hours treatment. Specimen size constant, I5/32 inch x 7/8 inch x 3 inches. So*Ss ,?
-. 1070
a e MI 0.01
3114 Aft &~
:S 0 wC Testsm ato05 000ý100 800 300 400100 100 300 400
8 100O, atlon of Test'hws A-49134
'00 FIGURE 22. COMPARISON OF TIME AND TEM-________ PERATURE EFFECT FOR NICKEL-COBALT-
IRON ALLOYS SHOWING HIGH RESISTANCE TO00. ATMOSPHERIC CORROSION( 2 1 )
Specimen sis. constant, 5/32 inch x 7/6 inchx 3 inches.
containing 45Ni, Z5Coll 7. SF., 20Cr, 2. STi.These data are shown in Figures 19 through 22 andTable 3. Additions of aluminumr, definitely increase
im j 400 the oxidation resistance lowered by additions ofAwam of4W. Awwmolybdenum (Alloys 2913 and 3115). The effect
FIGURE 21. EFFECT OF TIME ON PROGRESS of titanium can be judged by comparison ofOF OXIDATION OF MODIFIED K42B ALLOYS Alloys 3007 (normal KC42B) and 2870 (K4ZB minus
AS RVEALD B TOTL WEGHTLOSSFOR its normal titanium content), which generally in-AS0 REVEALED BY0 TOTA(L WIH LS O dicates a detrimental offe'#t due to titanium, but
100,200,AND400 OURS 21 )not at all times and temperatures of the test.Data for 900, 1000, and 1100 degrees centigradeare included. Specimen @ise constant, 5/32 Treche and Wators( 2 2 ) reported the oxidationinch x 7/8 inch x 3 inches. rate at 1900 F of a now nickel-base supetralloy, TaZ8
![Page 17: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/17.jpg)
14
TABLE 3. SUMMARY OF DATA FOR OXIDATION TESTS INCLUDING ChEMICAL ANALYSI AND MERIT NUMBER O1 ALL THE METALSAND ALLOYS SUBJECTED TO TEST(Z1)
Tests atTests at 600 C Teots at 900 C Tests at 1000 C 1100 CChemical Composition Me rit Weihb, Merit Weight Merit Weight Merit Weight
Alloy NI Co aF Ti No. Scale(e) Chane No. Scale Change No. Scale Change No. Chanse AlUoy
3108 13 47 7.5 2.5 20Cr Al I C.a. +0.05 2 ca.o. +0.031 Z c.a. :0.016 4 -0.461 50l3114 46 5 ?.75 2.5 19 Cr S Al 2 c.a. +0.019 3 ca.. +0.028 3 c. .- 0.061 2 -0.124 31142870 48 25 7.0 ... 20Cr 3 c.a. +0.021 4 c.a. +0.032 6 c.a. -0.536 S -2.%544 2070NICr IV 00 ........... 20Cr 4 c.a. +0.02 2 c. a. +0.031 4 c.a. .0.11 3 -0.404 NiCr IV3113 46 25 7.5 Z.5 19Cr 2. SAl S c.a. +0.025 c.,a. +0.039 5 c.s. -0.320 7 -3.391 31133007(K42B) 45 25 7.5 2.5 20Cr 6 c.a. +0.030 32 c.a. -0.112 9 c€.. -3.241 6 -4.563 (K422)310? 23 47 7.5 2.5 20Cr 7 c.a. +0.032 11 c.a. -0.071 10 c.s -2.41 9 -4,392 (Z469)2916 44 24 7.5 2.5 37Cr Mo 6 c.a. +0.034 9 c.a. -0.047 7 ca. .0.63 11 -9.535 29163009 44 24 7.5 2.5 17Cr5 W 9 c.a. +0.034 10 .... -.0.065 a 60a. .0.906 6 -4.065 (291013006 47 30 7.5 2.5 13Cr 30 c.a, +0.01 6 .... -0.033 3 cs.a. -2.611 10 -7.070 (41b)2i46 26 54 7.5 2.5 10Cr II c.a. +0.098 15 90s. -3.20 13 c.a. .4.457 12 -13.605 2068Nickel 32 c.a. +0.3171 ? ca.. +0.5311 1 c.. +1.034 1 +1.93 Nickel2920 77 20 ....... 3sO 13 C.a. +0.194 6 C.a. +0.058 12 60.. -3.994 29202935 30 50 10.0 ... 6Cr 2 Va 14 c.a. +0.240 18 c.s. -9.35 26 c.a. -18.33 9.... 2913115 56 30 7.5 2.54 Mo 2.5 Al 35 95 a, +0.260 16 C.a. -5.46 3& c.s. -7.47 13 -14.16 31t518-8 A .. 74.0 ... 10Cr 16 c.s. -0.342 14 c.a. -2.324 14 c.s. -4.637 3.-6
Konal 73 17 7.5 2.5 17 50 s. -0.407 20 e.a. -4.67 19 c.g. -9. 3z . Konal3004 58 27 10.5 4.5 36 e.s. -0.474 16 c.s. -3.93 is e.s. .4.063 ..... (K3Z)3008 15 40 42.5 2.5 19 c.a. .0.500 13 50.. -1.51 15 90s. -5.233 (K56)3109 49 26 7.5 2.5 ISW 20 S0a. -0.614 20 c.s. -4.67 21 c.s. -9.537 ..... (2907)2908 53 29 7.5 2.5 8W 21 c.a. -0.866 26 C.O. -6.29 23 e.a. -31.14 2908X52 40 41 16.0 2.5 22 c.s. -0.916 37 c.s. -3.9 22 cs. -11.014 "1. 22909 56 30 7.5 2.5 4 W 23 90s. -1.090 23 c.s. -5.33 26 c.I. -32.29 29092912 53 29 ?.S 2.5 SMe 24 cs. -1.117 22 c.s. -4.73 20 e.a. .9.17 ..... 29123005 58 32 7.5 2.5 25 65. . -i.2Z5 27 c.a. -6.76 27 e.s. -32.40 .(3(2)2567 27 54 IS,0 4.0 26 70 .. -1.396 ZS c.s. -6.03 15 e.a. -11.634 26673113 46 25 7.3 2.5 19 Me 27 c.s. -1.410 19 e.s. -3.95 17 e.g. -7.631 14 -17.619 (2911)2914 30 56 7.5 2.5 2 Va 28 75 .. -1.452 29 c.s. -13.4 29 c.s. -17. a(b) ..... 29142913 56 30 7.5 2.5 4 Me 29 c.s. -1.573 24 c.g. -5.61 24 c.g. -31.40 2913Cobalt 30 c.s. -10.0713 30.30 ........... ..... Cobalt
(a) c.a. - completelyadherent.c. s. - completely scaled.
(b) 200 bours.
Specimens size constant, 5/32 inch x 7/8 inch x 3 inches. Values recorded indicate total change in weight in gram.n after 400 hours.
(Ni-8Ta-6AI-6Cr-4Mo-4W- 2. SV- IZr- 0. 1ZSC). 20 tFigure 23 shows the results, and compares the Ir NI-ST@-6Cr-6 -4M0-4W'.oxidation rate of the new alloy with the oxidation IZr-0.125Crate of Ran6 41 and Nicrotung, which were tooted 10 Y ....41simnultaneously with the experimental alloy. Data ,on Nichrome are also included. a . Nlccrme(o )
The microstructures of the experimental --
NASA alloy, Rene" 41, and Nicrotung after a ZOO- 4 o000hour oxidation test at 1900 F are shown in Fig-ure 24(22). A relatively uniform layer of oxidescale is seen on the surface of the Reng 41, andpartially on the Nicrotung. None is visible on the / 2NASA alloy, but it was reported that the scaleprobably spalled off during cooling between 800and 600 F. Between the surface oxide and the un-affected material is a depleted sone which evi-dently varies in thickness a great deal among the so s 00 200 400 a0three alloys shown here. In addition, consider- Tim,hours A- 491able intergranular attack has occurred in theReni 41 and Nicrotung. FIGURE 23. WEIGHT GAIN PER UNIT AREA AS
A FUNCTION OF TIME AT 1900 F FORAn interesting study of the oxidation behavior SEVERAL NICKEL-BASE ALLOYS(2 2 )
of fine wires was made by Johnson, et al.(2 3 ) (a) From: Barrett, C. A., Evans, E. 3,Figure 25 and Table 4 summarize some of their and! Baldwin, W. M., Jr., "Therm.o-findings. One interesting item is the apparent in- dynamics an Ki.etics of Metals andcrease in specific oxidation rate with increase in Alloys - High-Temperature Scaling ofwire mins. More is said about the effects of sec- Ni-Cr, Fe-Cr, Cu-Cr, aMW Cu-tntion size in the section of this report on inter- Alloys", Final Technical Report, Marchgranular oxidation, to November, 1955, Case Institute of
Technology (December, 195S).
![Page 18: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/18.jpg)
12
- ~Surface
.Depletion
,~do,
matri
NNArSAn aloyRee 1 -615
FIGUE 24 ICOSTUCIUE OFOXIDTIO TES SPEIMESuIN VCINT F XOESURFAE AFER ZO HORS EXOSUR ATx900e
750XThephtogaps hv.bee rducd pprxiatey 0 pr eninpleiontv.
![Page 19: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/19.jpg)
400 13400 60 mil 1 TABLE 4. PARABOLIC RATE LAW CON-
STANTS, k, FOR OXIDATIONInconel 702 2.0 mil-- OF FINE woEmS( 2 3 )
300 I.Omil,,,_ Va. .I.._.,_.._:._. _.
WireDiameter, k x 1011
200 milo RenA 41 Elgiloy Inconel 702
At 2000 F
1 05 13 2.1 --
1.0 21 10 14
1800 2.0 37 11 23X)1800 2000 5.0 45 24 27
S1 Test Temperature, F
At 1800 F
0.5 7.5 0.91 --
Soo 1.0 9.2 3.0 1.7
5.0mi 2.0 11 6.0 2.05.0 26 13 6.7
500At 1500 F
(n 400'4 r 2.0mi 1 0.5 0.84 0.28 -
0Am1.0 0.16 3.? 0.152.0 0.84 3.1 1.2
5.0 3.1 1.8 2.8
Tee Tmpeatre eliA ,15 |0 - P'•-
1500 10 0(
I '.I
FIGURE 25. OXIDATION OF FINE WIRE OF f ' ---
VARIOUS .JIAMETERS AFTER 10 MINUTESEXPOSURE TO AIR" .,. "
After Johnson, et al. (23) ;P odd or
Data on the oxidation resistance of several bo
cobalt-base alloys are given in Figures 26 through30, and in Table S. Some early work by Eckerand Huffman( 2 4 ) is shown in Figures 26, 27, and28 for Alloys S-816, Haynes Stellite Alloy 21, andHaynes Stellite Alloy 31, respectively. Data from FIGURE Z6. RATE OF OXIDATION
Eberle, st al. ,(25) are superimposed on Figure 27, OF S-816 SHEET( 2 4 )
and ahow good correlation with the data of Eckerand Huffman. In all cases, the results are re-ported in terms of weight gain. noted, and further characterisation of the oxida-
tion rate was not possible. Note also that the
Weight gain data for L-605 and X-40 (same as magnitude of the weight gain is much less than re-
Haynes Stellite Alloy 31) were reported recently ported by Ecker and Huffman.( 2 4 ) At tempera-by Wlodek.( 2 6 ) Figures 31 and 32 show the results. tures of 1600 F az4 below, L-605 also showed
In the case of X-40, very erratic behavior was erratic behavior. However, after 1000 minutes
![Page 20: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/20.jpg)
_o __7__1_1__ 14 __ __ _ __ _
ki~w.weV Cwobtmou
D a- 11110 Or ycl~ 0 0- 2000 o& -SMF £-1900F
-141fic0 "ir'ol 1"(146" & _clw
47 1 i1
FIGURE 27. RATE OF OXIDATION OF FIGURE 28. RATE OF OXIDATION OFHAYNES STELLITE 21(24,25) HAYNES STELLITE 31(24)
321
eli 24 - -W~i52(Ref~runc26
~20 0.10 offe S ch,.mumm11700 F)
12 in .. VAQJIEftLJ. -cai
Teme~h0uv
FIGURE~~S 29.eftfflc OXDTO 2EITNE FTO FGR 08FFC)FAUIU NCOBALT-1A0 SUE.IJY COMPARE CHOMU COTN NTH 0XDTO
WITHTHATOF TO NW NIKEL, BAE RAE OFAF-9 MOIFICT0O00 2 8
SUPERALLOYS(12 a 28) ofe onho I0-h tIt Tad o in tIlar
170ad20 .Secmnes,0 noimz0 n og
![Page 21: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/21.jpg)
10.0
2200 F
2100 F2000 F
I.Oi-1900F
* ~1.0 I GOF
1700F
,160 oF
1400F
S0.10-
0,0!
0.01,0 100 1000 0),O
Time, minutesFIGURE 31. LOG-LOG PLOT OF WEIGHT GAIN DATA FOR L,-605( 2 6 )
10D
x-40 2000F
1900F
1.0 I700 F
1600 F
1400 F
S0.1-
0.0.
10 100 000
Time, minutes
FIGURE 3Z. LOG- LOG PLOT OF WEIGHT GAIN DATA FOR X-40(2 6 )
![Page 22: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/22.jpg)
16at 1700 F or after 10 to 100 minutes at higher MacFarlane, Pitler, and Reynolds (Figure 30)temperatures a reproducible parabolic rate was showed that aluminum and chromium are bene-observed. The erratic behavior of L-605 was ficial to the oxidation resistance of a cobalt-baseascribed mainly to extremely heterogeneous scale alloy. (29) The alloy used as a basis was AF-94,distribution, Some areas of specimens oxidized a cobalt-base alloy containing normally 0. 12C,at 1'•00 F for example, were virtually free of 15Cr, lONi, 5Mo, 1OW, l(Cb + Ta). The oxidizedoxide. X-40 also oxidized heterogeneously, but specimens were descaled in a hot caustic solution,the ýause seems to have been preferential oxida- and thus the results are shown in terms of weighttion in areas containing high-tungsten M6C-type loss. The loss is reported as a percentage, butcarbide phases, as well as other variations in the data can be considered within their own frame-chernimal composition, work as the specimen size was held constant
The main scale product on L-605 was found throughout (0. 500 in. in diameter x 0. 500 in. long).
by Wlodek to be a spinel of the form CoCr 2 0 4 . INTERGRANULAR OXIDATIONDuring parabolic oxidation, smaller amounts ofCr 2 0 3 and CoO were found. At a temperature of A comparison of the results of oxidation ex-
2200 F catastrophic attack seems to have been as- periments using the weight-gain or weight-loss
sociated with the formation of a low-melting scale method may not indicate the full extent of oxida-
of CoW4 , C0304, COO, and CoCrA4. Generally, tion change. Superalloys, particularly the
the oxidation products found on X-40 were the precipitation-hardenable nickel-base family, are
same as for L-605, though a much smaller amount susceptible to intergranular oxide penetration.
of catastrophic oxidation hindered positive identi- While this type of attack may have little effect on
fication of CoW4. the strength of articles of large cross section, itcan be a serious problem in the case of thin sheet,
Measurement of the increase in total thickness foil, and fine wire. While it is possible for theof L-605 sheet indicates 0. 1-0.3 mil at 1200 F, general surface oxidation to be practically nil and0.2-0.5 mil at 1500 F, and 0.7- 1. 2 mile at 1800 F, of little importance in these thin sections, even aall for 50 hours.( 1 7 ) small amount of intergranular penetration may
J-1570 as reported lead to premature failure. For example, penetra-by Dempsey(27) arleo T 5. a ohese tion of 2 mils from each side of a 15-mil sheet
tests, the specimers were exposed for 16 hours at would reduce its load bearing cross section by2000 and 2200 F, descaled, and then exposed for about 27 per cent. Penetrations of this order,another 16 hours. e. g., 1-2 mils, are not unusual for the super-
alloys. Fortunately, intergranular penetrationTABLE 5. CORROSION BEHAVIOR takes place only at relatively high temperatures.
OF ALLOY J-1570( 2 7 )Time-temperature-penetration curves have
been obtained for Rene 41, as shown in Figure 33.(30)Weight Loss, g
Speci- Tempera- During First During Second . , . , ,men ture, F 16 Hours 16 Hours .0028 -- -- -1-25hr h
1 2000 0.1199 0.2418.02Z 2000 0.104)h
3 2200 0.4527 1.0515 . .0020 - 2000 hour exposure
Note: Specimen size was 1/4 in. x 1/4 in. x • 0016 ti -3/4 in. 101h
Information on the oxidation resistance of .0012 .2.5 tw
SM302 and WI-52 cobalt-base superalloys is Cshown in Figure 29.(28)* Data previously shown .0006 -
for nickei-bas-t alloys IN- 100 and SM200 are in- 4cluded for comparison purposes, as the tests ap- -.0004 - -parently were conducted under identical conditions. / /0.51W
".00001'140100*Further infornmation on the oxidation character- o1400 1500 1600 700 180 100 2000istics of SM302 was recently published by E. J. Fxposurs Temperoture, FFelten and R. A. Gregg in Transactions of the A-49131American Society for Metals, 57, 804-822 (1964). FIGURE 33. DEPTH OF OXIDATION VERSUSIn ade ion, NASA investigators J. C. Freche, TEMPERATURE FOR RENi 41(30)R. L. Ashbrook, and G. D. Sandrock recentlypublished information on the oxidation resistance The curves show the depth of intergranularcf cobalt-tungsten alloys (Trans. ASME, Series B, oxidation. The depth of uniform oxidationFebruary, 1965, pp 9-20). is negligible.
![Page 23: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/23.jpg)
17In this figure, it can readily be seen that inter- Intergranular oxide penetration affects notgranular penetration increases greatly with in- only the tensile and stress- rupture properties bycreasing time and temperature. For example, the reducing the effective cross section, but it alsotime for 1 -msl penetration (2 mile total, ! mil can be expected to be detrimental to the fatiguefrom each side) to occur, changes from about 1000 strength because the "tongue" of corrosion willhours at 1500 F, to 10 hours at 1750 F, 2.5 hours . as a notch.( 3 2 )at 1850 F, and about 0.8 hour at 2000 F. Figures 35 and 36, from SimeniS 3 3 ), show
Similar, though not identical, results were ob- the intergranular attack on several nickel- andtained by Childers and Koriagin( 3 1), as shown in cobalt-base alloys. Figure 35 gives the resultsFigure 34. These results are for oxidation at sea of a 1-hour exposure at various temperatureslevel, and somewhat less severe attack may occur from 1600 to 2200 F. Figure 36 shows the resultsat reentry altitudes, according to preliminary data of ten 1-hour cyclic exposures at these same tern-presented in Table 6. On the other hand, the ef- peratures. The data are for a single side andfects of dynamic pressure and velocity were not would be doubled if attack was present on bothevaluated. Consequently, the data obtained cannot sides. It is interesting to note that the solid-be used to determine the extent of attack during solution-hardened Hastelloy X gives lower oxideactual reentry conditions, penetration than the precipitation-hardened nickel-
base alloys at all temperatures during the cyclictest.
Figure 37 gives the oxide penetration after100 hours in slow-moving air for three Inter-
0348 hr national Nickel Company alloys and AMS 5537S0.0036 24hr (L-605 cobalt-base alloy).(34) In these tests, the
U aluminum-bearing alloy, Inconel 702, showed less
intergranular penetration than did the titanium-0.002 bearing alloy, Inconel X.100 hr 10 hr Ignatov stated that additions of 4 per cent
0.00. /aluminum to 80-nickel- Z0-chromiumn alloys pre-I hr vents intergranular oxidation. Additions of tita-
nium on the other hand increase the intergranular
A 0 oxidation. (5) The difference lies in the structure1500 1600 1O0 la0o MI 2000 of the oxides formed and the fact that Ni 3 Ti lies in
Temperature, F a-4s0 the grain boundaries. Aluminum forms the dense,closely packed A12 0 3 structure, whereas titanium
FIGURE 34. EFFECT OF TIME ANDTEMPERATURE ON OXIDE PENETRA- On* 1AlIyV25TION OF RENE 41 IN STILL AIR( 3 1 ) / lI.uveupo w
TABLE 6. EFFECT OF AMBIENT PRESSURE Km xON OXIDATION OF RENE 410(1) • ost i--'43
Exposure Ambient Depth ofTempera- Time of Pressure, Penetration,ture, F Exposure rmm Hg in.
2000 100 min. Sea Level 0. 00084
2000 100 min, 0.090 0. 00080
2000 1800 hr. 10-4 None
Information on oxide penetration is of greatimportance now that increasing use is made ofthin sheet for structural applications at high tem- =peratures. It is also important in the heat treat- o am 1= toment of sheet. Temperatures of 1950 to 2150 F Tem.oe-ste. Fare regularly used in the solution treatment priorto aging. Thus, finished sheet may be susceptibleto penetration during heat treatment. Aging tem- FIGURE 35. DEPTH OF ATTACK AS Aperatures are too low to be of importance to the FUNCTION OF TEMPERATURE FORproblem at hand. VARIOUS ALLOYS(3 3 )
![Page 24: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/24.jpg)
18
forms the defect (anion deficient) structure of-- rutile, TiO2 . Oxidation of nickel-chromium alloys
Toe I-himo, exp*tu normally proceeds by diffusion of the metallic ionsI Mow 25through the oxide to the outer surface, where they
Scombine with oxygen. Accordingly, diffusion of
1 metallic ions to the oxide-metal interface is therate-controlling process. However, the defect
£i .__ structure of rutile permit. a greater proportionof oxygen diffusion inward to the interface, result-
1x1:1 ing in a higher rate of oxidation at the oxide-metalinterface in titanium-bearing alloys than in
.... R... --- A aluminum- bearing ones.
Dukes, et al., studied the oxidation behavior10- of a nickel-base alloy, Inconel 702, and a cobalt-
____ base alloy, Haynes Alloy 25 (L-605).( 3 5 ) The re--*a sults of these studies are given in Figures 38 and
SXa39.(35) Figure 38 illustrates the excellent oxida-__ _tion resistance of Inconel 702.
When wires and sheet of 6-mil thickness are__intergranularly attacked on all surfaces to a depth
of 2 mils, the sheet retains one-third its originaleffective cross-sectional area, whereas the wire
J._ retains only one-ninth. Figures 40 and 41 illus-amo- trate the effect of oxidation on the room-
TOmpWatt, F temperature strength properties of Reng 41 andInconel 702 wire, respectively, after exposure in
FIGURE 36. DEPTH OF ATTACK OF VARIOUS static air for 5 minutes at various elevated tern-ALLOYS CYCLED TEN TIMES TO THE peratures. (23) These curves show that the ef-INDICATED TEMPERATURES( 3 3 ) fective cross section of fine wires held at high
A0
Sheet samples exposed for 100hours in slow-moving air at
.0 teperatures shown
.015
I .(
S1~L605 cobamlt-lban
loInconel "
0 Inconel
Inconel 702
0.01 . ....am 1100 t200 o300 3400
Temperature, F A-ee11?
FIGURE 37. DEPTH OF PENETRATION VERSUS TEMPERATUREFOR SEVERAL NICKEL- AND COBALT-BASE ALLOYS( 2 7 )
![Page 25: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/25.jpg)
19
Mef 0.4
0.3
g~ 0-Uniform surface scaleS
X -Total attock(uniform + intergr nular)
0.75
0.5 2 0 r0 T5000 F 0 60
Hours of Exposure A-49154
FIGURE 38. OXIDATION BEHAVIOR OF INCONEL 702 SHEET EXPOSEDTO AIR AT ELEVATED TEMPERATURES( 3 5 )
temperatures can be entirely consumed by oxida-~ -~- ____________ tion. Table?7 shows the effect of oxide penetra-
T. A0M F 0 - UNFM tffe ,wam cll tion on the short-time tensile strength of 0. 010-- - '~ *' *'~-- -inch-thick Rene' 41 sheet.( 3 6 ) Several items in
IS -r -3 2 this table are of interest. First io the difference[10 - T200: -- "I in strength levels, in tension, as a result of heat
+-R -IOFtetet h low-temperature solution-treat-and-age sequence, A, results in significantly
higher tensile properties than does the higherC0
;01 TIOM F temperature cycle, C, when tested as heatF -- ---- ---- --. treated. When these specimens were soaked for
i 10-20 hours at 1800 F prior to testing, this dif-------------------- 0 ference in strength was very much lessened. On
the other hand, when they were soaked for 10-20----------------- T~eO J hours at 2000 F before testing, there was again a
ISM rlarge difference in strength. Also of interest isao1 the fact that the unaged specimens, B, were at
"Switelleast as strong as the aged specimens when testedafter soaking for 20 hours at 2000 F.
Wlodek(2-6 ) found that L-605 was oxidized in-FIGURE 39. OXIDATION BEHAVIOR OF tergranularly when exposed at temperature* fromHAYNES ALLOY 25 SHEET EXPOSED TO 1600 to 2200 F. A more even distribution of sub-AIR AT ELEVATED TEMPERATURES( 3 S) scale oxidation occurred when the specimen was in
![Page 26: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/26.jpg)
20
1500 F-o IO100 F
% lgial U ýSot ýOrIgia U TS at=M-0-ro m temosmitura
180 F-- -7 180
0ý -l - M -.
200 F 2000 F
*C 070c0
at room temperatwre - - I
d -
0/0
lot Wire Diameter, mile
Wire Diameter, mi I$ A-49443 FIGURE 41. EFFECT OF INCONEL 702 WIREDIAMETER ON LOSS IN STRENGTH ANDDUCTILITY AFTER HEATING IN STATIC.FIGURE 40. EFFECT OF RENE 41 WIRE AIR FOR FIVE MINUTES( 23 )
DIAMETER ON LOSS IN STRENGTH ANDDUCTILITY AFTER HEATING IN STATICAIR FOR FIVE MINUTES( 2 3 ) the aged condition than when in the mill annealedcondition. As-cast X-40 suffered internal oxida-
TABL 7.ROOM TEPERAUREMECHNICL PRPERIES tion mainly along the interdendritic areas. TheTA OE F ROOMTEM41RAFTERE SOKATEEVHATIA OED average depths of internal oxidation in L-605 and
TZMPERATURES( 3 6 ) X-40 observed in Wiodek's work and in other workUltiate(cited in Wlodek's report) are shown in Table 8.
float- T:nut1 Yield Elonga-Trat Sr at Strongt*b tion,ment(a) Test Condition kit kat TABLES8. AVERAGE DEPTH OF INTERNAL OXI-
A No Soak 173 140 aDATION IN L-605 AND X-40(2 6 )A Soaked 16007J, 10 hours 129 75 9 ____________ ________________A Soaked 2000 F, 10 hours 126 76 14A Soaked 1600 F, 20 hours 117 70 6 Depth of -Oxidation Per Side, mileA ScAked 2000 F, 20 hours 112 74 133a13 Soaked 2000 Fr, 20 hours 115 611 14 Alloy Temp. F 24 hr 100 hr 400 hrC No Soak 131 124
C Soaked 15007F, 10 hour@ 110 77 9 L-605 1600 0.1 0.6 0.8C Soaked 2000 F, 10 hours 76 59 5C Soaked 16007F, 20hours 106 72 61800 0.7 1.3 1.7-C Soaked200FZOOOr hours 64 54 2000 0.9 2.0 2.8
(a) flest-treatment, c( 9od F2 015,. .A - Solution treat 15 ,age 1400 F51 -solution great 3950 F, no age X-40 1600 0.2 0.5 1.0CSolution treat 2150 F, age 1650 F. 1800.8 1.5 2.2Mb Calculated usin maeiltikesbfr ea oiia hcns 000 .6 3 .0. 010 inch). igmtra hcns eoesa oiia hcns 0 01 . .
2200 1.3 2.2 3.7
![Page 27: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/27.jpg)
21Alloy Depletion Effects
hL
Intergranular oxidation is preceded by alloy -25depletion ahead of the advancing oxidation as seen I? ,ý hrin Figures 38 and 39. The compositional gradientthat is produced can act as the driving force for 4514- 30h
continued metal-ion diffusion. The depleted son*also is weaker than the basic alloy, particularlyin precipitation-hardenable nickel-base alloys 1.4 5 Nwhere chromium, aluminum, and titanium are 1.2preferentially oxidized because of their relatively • 1.0high affinity for oxygen. Loss of titanium and alu-minum content is particularly detrimental to 0.8 25 hrstrength properties.( 3 0 p 32) 0 0.6
Malarnand and Vidal made a study of alloy de- 0.4 100 hr
pletion by oxidation for various nickel-base 0.2- 300 hralloys.43 7) Their results for Nimonic 80 andNimonic 95 are shown in Figures 42 through 45. &0Composition was determined apectrog raphic ally. 2,8
20 OOC- 50CP502C
, 19 2A -
17 Zo 1
700 C 750 C 850C 900 C1.64
5 1.2 - 1.0
,.0 -oo 0A,
a 0.6 Depth in Micron A-49149
0.4FIGURE 43. VARIATION OF CHROMIUM,
0.2 ALUMINUM, AND TITANIUM CONTENTS
WITH DEPTH BELOW THE SURFACE IN700 - C1 -NIMONIC 95 ALLOY OXIDIZED IN AIR AT
2.4 •800 C FOR 5, 25, 100, AND 300 HOURS( 3 7 )
2.2
2.0-Figure 42(37) shows the depletion of chro-
1.8 mium, aluminum, and titanium in Nimonic 80
1.6 after 300 hours' exposure at various temperatures.1.4 Figure 43(37) shows the depletion of Nimonic 95
_- alloy as a function of time at 800 C (1475 F). The-1.2 compositional gradients are quite steep even at
short times. Figure 44(37) shows data on the de-1.0 20 pletion of various elements in Nimonic 95 after
0.8 - 20 40 60 60 I00 120, 300 hours at 800 C (1475 F), and the attendant de-Depth in Microns £-49144 crease in hardness; note that cobalt is not de-
pleted. Figure 49(37) is interesting because itFIGURE 42. VARIATION OF CHROMIUM, represents a treatment often used on commercialALUMINUM, AND TITANIUM CONTENTS hardware such as turbine blades. After machining,IN NIMONIC 80 ALLOY OXIDIZED IN AIR these parts are "skin annealed" in a salt bath toAT TEMPERATURES BETWEEN 700 AND recrystallise the cold-worked areas.( 3 7 ) A corn-900 C( 3 7 ) mon practice is to heat the parts at 1080 C (197SF)
![Page 28: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/28.jpg)
I
22Chromium -20
16 V115-
.Titnium -. .4I- " . _°
2 1.2
2.2oAlu 2-m 2.,
2.4
2.-12 i* 1,6
10. 1.4Hardness 1 _2____1_1_1___ __1
°s0 0 I + +. + 1+ 0 102030405060708090101101201301401
0.6 Depth in Microns A-4S135
FIGURE 45. VARIATION IN CHROMIUM,+ ALUMINUM, AND TITANIUM CONTENTS
=L0 02h r+z 2 IN NIMONIC 80 ALLOY AFTER "SKIN0 0 2D M 40 50 60 70 8D 90 1POO ANNEALING" FOR TEN MINUTES AT
Depth in Microns A- 49144 1080 C (1975 F)( 3 7 )
FIGURE 44. VARIATION OF CHROMIUM,COBALT, TITANIUM, AND ALUMINUM by diffusion of Cr+3 along grain boundaries andCONTENTS AND ACCOMPANYING HARD- through the nonthickening alumina layer. InNESS OF NIMONIC 95 ALLOY OXIDIZED Hastelloy X, a film of amorphous silica acts likeIN AIR AT 800 C FOR 300 HOURS( 3 7 ) the alumina film in the Rene" 41, depleting silicon
from the alloy, and requiring that further oxida-tion proceed by diffusion of Cr+3 and Ni+Z.
for 10 minutes. Figure 45 shows that metal downto a depth of 100 microns (0. 004 in. ) is affected In X-40 and L-605, Wlodek( 2 6 ) found that theby depletion, alloy depletion effects were not pronounced enough
to be observed reproducibly by etching. When ob-Wlodek's recent work( 1 8 # 16) on the oxidation served, the depth of alloy depletion was roughly
of Hastelloy X, Reng 41, and Udimet 700 con- equivalent to the depth of internal oxidation.siders subscale reactions involving alloy depletionand internal oxidation. In Reng 41, Wlodek notes OTHER SUBSURFACE OXIDATIONthat the apparently intergranular attack (see Fig-ure 33) below the scale does not follow prior grain Some nickel-chromium-base alloys are sub-boundaries, but penetrates along a network of ject to subsurface preferential oxidation, some-newly formed subboundaries. He refers to this times called green-rot. This has two distinguish-attack, which occurs with a different morphology ing characteristics, namely, that a fracturedin Hastelloy X and Udimet 700, as internal oxida- surface has a definite green color, and that thetion. Wlodek found that in Rene 41 and Udimet 700 metal area affected is magnetic because of the lossthe oxidation process occurs in three successive of chromium. Although this particular type of oxi-stages: formation of a thin film of DA1 2 03, deple- dation is not usually found in the superalloys, it istion of aluminum from the alloy adjacent to the discussed here in order that it may be recognisedoxide/metal interface, and oxidation of chromium if encountered.
![Page 29: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/29.jpg)
23This form of internal oxidation in nickel-base oxidation occurred unless conditions permitted the
alloys is unpredictable, and no completely satis- dissociation of some CO to C and CO2 . Under thefactory model has been developed to explain its conditions of the experiments, the optimumoccurrence. Two general schools of thought exist. amount of carbon dioxide for producing internalOne ascribes the internal oxidation to the prefer- oxidation was 3 to 13 per cent. Catalytic actionential oxidation of chromium rather than of nickel accelerated the attack.in atmospheres that are oxidizing to chromium andreducing to nickel.( 3 8 ) Such atmospheres, of EFFECT OF STRESScourse, would exist only under special conditions,but this type of oxidation could also take place if Any discussion, however brief, on the prob-the ambient atmosphere fluctuated between oxidiz- lem of oxidation of superalloys should includeing and reducing. some mention of the effect of stress on the oxida-
tion behavior of the alloys. It is difficult, how-Another school of thought holds that internal ever, to present specific data because of the in-
oxidation takes place most readily under a surface dividual nature of the response of each alloy to thethat had been previously carburized. It is con- combined effects of oxygen, temperature, andsidered that the chromium carbides formed as a stress. Data of this type are scarce, and dataresult of the carburization are preferentially at- from different studies cannot be compared satis-tacked. There have been many observations, factorily because of the wide variety of testingmade under industrial conditions, that tend to conditions. Data are sometimes generated ad hocsupport this viewpoint, to satisfy a specific need, application, or design
factor.It was concluded from a series of experiments
by the International Nickel Company that the Some general ideas on the oxidation behaviorparameters for internal oxidation are not clearly of superalloys under stress were rut foath ia thedefined.( 39 ,40) It was found that internal oxida- work of Richmond and Thornton.(4 ) TaMe 9 andtion took place more readily in areas that had been Figures 47 and 48 represent data extreceed frisspreviously carburized, but that carburization was their work. The depth of penetration ws ete•r-not a prerequisite. Areas not previously carbur- mined by observation of metallouc specirnem.ized also were attacked; however, ambient atmos- The most significant finding ws t, at eachphere was also found to be an important considers- temperature level, oxidation peanwod at a coan-tion, although its specific effect was not stant rate with increasing stamatil a certairndetermined. Electron-probe microanalysis critical stress level was reocbed at which oxide-showed that the chromium content of the oxide and tion proceeded much more mapklly. Table 8 simr-carbides of an oxidized specimen were indeed marires these data. Figures 47 and 48 show datahigher than the matrix (see Figure 46), thus sup- plotted for Hastelloy Alloy R235. Similar curvesporting the concept of chromium depletion from can be drawn for the other alloys. In the exam-the matrix.(4 0 ) However, these studies also ples shown, HastelloyAlloyRZ35 begins to undergoshowed that similar specimens could be made to accelerated oxidation at 1500 F when a stress leveloxidize internally, or not, by varying the tempera- of about 23, 000 psi is reached. At 1600, 1700, andture and composition of the ambient atmosphere. 1800 F, the critical stress levels are about 15,000,When carbon monoxide gas was used, no internal 12,000, and 5,000 psi, respectively.
Carbon Monoxide The increased oxidation rate can be explainedOuter Block in many ways, two of which are as foUows:
Layer Carbon Per cent Per cent (1) increased diffusion rates occur within the............... ....--- - ,Chromium Nickelor * 56 35 stressed areas, thereby increasing the frequency* 40 with which metal and oxygen react and (2) at theOxide, * E9
a so " i TABLE" 9. STRESS AT WHICH DEPTH O OXIDE PENETRATIONBIEGAN TO INCREASE R.APIDLY WITH STRESS IN
Owl doSEVERAL NICKLL.- BASE ALLOVS04 1
1
Ca -. id 28 64 78res, .... .aCarbides~m do. OR d•- • O ? •...... .,.,,zm...
W, o?. A,.,. 5 . .D .pt of E.,..£ F.. Maa....... .phi, I Oid.dSm ml SP le Oxilde hlespierdlt-ro Penet rati|on
Al£loy 20 Sol. 0 00 £o 0 0oo £00 £00 £0oo 00 00(nickel -chromim)70 10.000 $,S0o 1,a" £10 10,000 '1.000 100A-4e913e Hastel£ oy RU|' ,1.OZ , £0000 0 4.. [ 0o 1000 21,000 iS,000 IZ, 000 $000
14SO £. O C1 0 ,0 £ 1 10 00 £1 I £0C 1110 11.00
|nC Z1 X to, 000 17,1so0 £M000 7000 .0,00 £1,0 " 0 iS. 0 7000?FIGURE 46. SCHEMATIC DIAGRAM OF £100 £0oo !£6$00 £200S £00 £160 I£s0ANALYSIS BY THE ELECTRON-PROBEMICROANALYZER( 4 0 ) ... ,.y.W ,000 ,.00 3.00 700 ,000 ,.00 1.000 ,0
![Page 30: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/30.jpg)
24
3. - 5,.15
2.0
i.8 1600 F 3.0 160 F
1 AA
-2.5 -
I- 'I"00 °l0 160
0. , 0 o ._ I i. 0 AA
WWIi Stroll, psi A - 4914 low"fe Slreis, Psi A-49150/
IF11111 Alp. MIOT Or AVERAGE DEPTH OF FIGURE 48. PLOT OF MAXIMUM DEPTH OF4CXTj1RNAL IM TION OF HASTELLOY R235, OXIDE PENETRATION OF HASTELLOY R235ot VICRATURES AS A FUNCTION AT FOUR TE0 MTURE AS A FUNCTION
ITIIiI~jI!|OF STRESS(41)bi.po0u.0 time for all specimesn was 100 hours. Exposure time for 0ll specimens was 100 hours.
critical applied stress the rate of metal deforma- produce accelerated oxidation roughly corre-tion just exceeds the rate of growth of oxides. sponded to the stress necessary to produce I perProtective oxides normally occupy a greater vol- cent extension in 100 hours.urse than the metal they displace, thus coveringthe metal with a self -healing layer that is in corn- Stress also is important from the standpointpression. If the metal underneath in being of spelling. Although the surface oxides on mostelongated at such a rate that the volume of oxide superslloys are tough tightly adherent layers thatformed is not sufficient to keep up with the rate of resist epalling, extensive deformation can produceexpansion of the metal surface, the oxide will no sufficient *hear at the metal-oxide interface tolonger be protective: fresh metal will be exposed cause cracking and separation.(14} Under these
as oxidation proceeds. In this regard an interest- conditions oxidation is rapid as fresh metal is con-ing observation was that the minimum stress to tinuously being exposed for further reaction.
![Page 31: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/31.jpg)
25
REFERENCES
(1) Tumarev, A., and Panyushin, L., "Scale (12) Preliminary Technical Data SM HighResistance of Alloys of the Ternary System Temperature Alloys, Sierra MetalsNickel-Aluminum-Chromium", Isvestiya Corporation (1962).Vysshikh Uchebnykh Zavedeniy-ChernayaMetallurgiya, No. 9, pp 125-131 (1959). (13) Eiselstein, H., and Skinner, E., "Effect of
Composition on the Scaling of Iron-(2) Zima, G., "Some High Temperature Oxida- Chromium-Nickel Alloys Subjected to Cyclic
tion Characteristics of Nickel With Chromium Temperature Conditions", ASTM SpecialAdditions", Transactions American Society Technical Publication No. 165 (1954).for Metals, 49 pp 924-947 (1957).
(14) Kihlgren, T. E., "A Review of Nickel-Base(3) Phalnikar, C., Evans, E., and Baldwin, Alloys for Aeronautical Applications",
W., Jr., "High Temperature Scaling of International Nickel Company.Cobalt-Chromium Alloys", Journal of Elec-trochemical Society, 103 (8), 429-438 (1956). (15) Childers, M. G., and Simenz, R. F.,
"Clad Protection of Thin Sheet", Society of(4) Gulbransen, E. A., and McMillan., W. R., Automotive Engineers Paper 742E,
"Oxide Film on Nickel-Chromium Alloys", September 23-27, 1963.Industrial and Enaineering Chemistry 45pp 1734-1744 (1953). (16) Wlodek, S. T., "The Oxidation of Rene 41
and Udixnet 700", Transactions of the(5) Ignatov, D... and Shamgunova, R., "Mech- Metallurgical Society of AIME, 230
anism of Oxidation of Some Ni-Cr Base pp 1079-1090 (August 1964).Alloys", Iuvestiya Akademii Nauk, SSSR,Otdel. Tekhn. Nauk, Metall. I Toplivo, (3), (17) Rabensteine, A. S., "Oxidation Charac-pp 83-87 (1959). teristics of Various Structural Materials
for Ramjets and Heat Exchangers", Report(6) Ignatov, D. , and Shamgunova, R., PR 281-4Q-1, under Air Force Contract
"Structural-Kinetic Investigation into OxIda- AF 33(657)-8706, The Marquardt Corpora-tion Process of Nickel and Chromium and tion, Van Nuys, California (June 15, 1963).Alloys Based on Them", rssledovaniy& poZharoprochnym Splavam, 4, pp 346-351 (1959). (18) Wlodek, S. T., "The Oxidation of Hastelloy
X" Transactions of the Metallurgical Society(7) Kubaschewski, 0. and Hopkins, B., Oxida- of AIME, 230, p 177 (February, 1964).
tion of Metals and Alloys, Academic Press,New York, New York, Second Edition (1962), (19) Manning, C. R., Jr., Royster, D. M., and319 pp. Braski, D. N., "An Investigation of a New
Nickel Alloy Strengthened by Dispersed(6) Hagel, W. C., "The Oxidation of Iron-, Nickel-, Thoria"t, NASA Technical Note D-1944,
and Cobalt-Base Alloys Containing Aluminum", Langley Research Center, Hampton,paper presented at the 2nd International Virginia (July, 1963).Congress on Metallic Corrosion sponsored bythe National Association of Corrosion Engi- (20) "TRW-1900 A High Strength Nickel-Baseneers, New York, New York, March 1 -IS, Superalloy for Use at High Temperatures",1963. Preliminary Date Sheet of Thompson Ramo
Wooldridge Inc., Cleveland, Ohio(9) "The Nimonic High Temperature Alloys", (March 25, 1963).
Engineering Data, Henry Wiggin and Company,Ltd, Holmer Road, Hereford, England (21) Austin, C. R., 0"High Temperature Prop-(1960). erties of Ni-Co-Fo Base Age Hardening
Alloys", Transactions American Society of(10) Betteridge, W., and Franklin, A., "Develop- Metals, 24, pp 461-512 (September, 1936).
ment of Ni-Cr-Base Alloys for High-Temperature Application", Revue de (22) Freche, J. C. , and Waters, W. J.,Mktallurgie, Memoires, 5 pp 271-284 "Continued Investigation of an Advanced-(1956). Temperature, Tantalum-Modified, Nickel-
Base Alloy", NASA Technical Note D-1531(11) Wood, D. R., "Investnent-Cast Alloys for (April, 1963).
High-Temperature Service", Foundry TradeJournal, 106 (227S),663-668 (June 4, 19S9).
![Page 32: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/32.jpg)
26(23) Johnson, D., Newton, E., Benton, E., (2() Betteridge, W., "The Nimonic Alloys",
Ashman, L., and Knapton, D., "Metal Edward Arnold Ltd., London, 322 pp (1959).Filaments for High Temperature Fabrics",AeD Technical Report No. 62-180, under (33) Simoen, R., "This Test for OxidationAir Force Contract AF 33(616)-7294, Resistance", Product Engineering, 30 (17),Arthur D. Little, Inc., Cambridge, Massa- 48-50 (April 27, 1959).chusetts (February, 1962).
(34) Inco Current Data Report Number 5,(24) Ecker, L., and Huffman, 3., "Final Report International Nickel Company, New York,
on Investigation of Sheet Alloys for Turbojet New York.Engine Exhaust Systems", North AmericanReport No. NA-48-400 (July 1, 1948). (35) Dukes, W. H., Gosden, C. , Kappelt, G.,
and Mirti, A. E., "Manufacturing Methods(25) Eberle, E. . Hoke, 3. H., Leyda, W. E., for Insulated and Cooled Double-Wailed
"Development of Cast Iron-Base Alloys of Structures", ASD TR-61-799, I, Section I,Austenitic Type for High Heat Resistance and (1961).Scale Resistance", WADC Technical Note55-290, under Air Force Contract No. AT (36) "Strength Properties of Reno 41 After33(616)-2413, The Babcock & Wilcox Short Time Exposure to High Temperature-Company, Beaver Falls, PeAnsylvania Time Cycles", Report No. SRM 434,(January, 1957). Preliminary Data, Lockheed Aircraft
Corporation, Burbank, California(26) Wlodek, S. T., "The Oxidation of L-605 and (September 8, 1959).
X-40", Report R64FPDI2, General ElectricCompany, Cincinnati, Ohio (January 24, 1964). (37) Malanand, F., and Vidal, G., "Effects of
High Temperature Oxidation on the Surface(27) Dempsey, K. B., "Sheet Material for Service Composition of a Ni-Cr-Ti-Al Alloy",
to 2700 F", Research Memorandum No. 8, Comptes Rendus, 240 pp 186-188 (1955).Universal-Cyclops Steel Corporation,Bridgeville, Pennsylvania (January 13, 1956). (38) Spooner, N., Thomas, 3., and Thomassen,
L., "High Temperature Corrosion in(28) "SM302 High Temperature Cobalt-Base Nickel-Chromium Alloys", Journal of
Superalloy", Sierra Metals Corporation, Metals, 19? p 844 (June, 1953).Wheeling, Illinois (1962).
(39) Copson, H., and Lang, F., "Some Experi-(29) MacFarlane, R., Pitler, R., and Reynolds, ments on Internal Oxidation of Nickel-
E., "Investigation of Forged Cobalt-Base Chromium Alloys", Corrosions, 15 (4),Alloys for High Temperature Applications", pp 194t-198t (April, 1959).WAD, rechnical Report No. 56-327, underAir Force Contract AT 33(616)-2882, (40) Hopkinson, B., and Copson, H., "InternalAllegheny Ludlum Steel Corporation, Carburisation and Oxidation of Nickel-Pittsburgh, Pennsylvania (October, 1956). Chromium Alloys in Carbon Monoxide-Typzý
Atmospheres, Corrosion, 16 (12), pp 608t-(30) Lund, C., "Physical Metallurgy of Nickel- 612t (1960).
Base Superalloys", DMIC Report 153,Defense Metals Informnation Center, Battelle (41) Richmond, 3., and Thornton, H., "Oxida-Memorial Institute, Columbus, Ohio tion of Experimental Alloys", WADC(May 5, 1961). Technical Report 58-164, Part I, under
Air Force Contract AF 33(616)-56-19(31) Childers, M. G., and Koriagin, V. B., National Bureau of Standards (Juno, 1958).
"Light Weight Structures for Space Vehicles",Society of Automotive Engineers Paper No.420C, October 9-13, 1961.
![Page 33: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/33.jpg)
APPENDIX
ALLOY INDEX AND COMPOSITIONS
![Page 34: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/34.jpg)
A-1
TABLE A-I. ALLOY INDEX AND COMPOSITIONS
Composition, per cent Index
Allo,. Ni Fe Co C Mn Si Mo W Cb Ta B, Zr Ti Al Cr Other Page No.
80-201 (NiLhrome V) 1al. 0 28 -- 0.06 -- I, 12 . .. .. .. .. . 19.8 6,10,11,17
N 0 -2 0 + k A n * 1a l . 0 . 4 4 - - 0 . 0 5 1 . 7 6 1 . 0 9 . . . .. . . . . .. . . . . . 2 0 . 0 6
l i.i t4 ll . A ll y, fl Ia . I 0 . 0 0- 0 , 1 5 . . . . 5 .5 . .. . . . . .. . 2 . 5 0 2 . 0 1 5 . 5 1 7 , 1 8 , 2 3 ,2 4It 2 Is
Ii.mtoIlloy Alloy W IBal. -- -- 0. I . S25 5 0. 6 V, max 23H..ýtilloy Alloy X Dal. 20 1.5 1.10 . . 9,0 0.6 -- 22.0 8,9, 17,18,
22,23IN - 10 0 D a.il. 15.0 0 .1 0 . . .. 3.0 .... . 0.015 0.0 5 5. 0 5.5 10 1. 0 5, 161bi onllt 0 .1 7.91 -- 0.04 0.25 0. 37 .. .. .... .. .. 16.4 7,18
I n n, l (pr-- 1951),0 Bal . L 67 -- 0 06 0.23 0.32 .. .. .... .. .. 14. I 6,7lnmonl W(
6 ) Dal. 6. 5 -- 0.04 .. .. .. .. .... 2.4 0.6 IS. 0 7
tIcon(P X(2
) lDcl. 6.75 -- 0.04 0.7 0.3 .. .. 0.9 - Z. 5 0.9 15.0 1,7,17,18Incontl 702(( ) Dal. 0. 35 -- 0.04 0.05 0.20 .. .. ... 0. 70 3.40 15,6 7,13,17-20,
23K421 Btl. 7. 5 25 .. .. .. .. .. .... 2. 5 -- 20 9-11N ic ro t ing B ll . - - 10 . . . . . . . . 8 . . . 0 . 0 5 0 .0 5 4 . 0 4 .0 12 1 1 , 12
Nin,-n•, 75 1a 1. -- -- 0. 12 .. .. .. .. .. .. .. . 0. 5 -- 20 4,6,7Nio•,om, 80 13a1. -- -- 0.08 .. .. .. .. .. .. .. .. 2.4 1.5 20 4,21,22
N i , , , o , 8 0 A D a l . . - 0 . 0 8 . . . . . . . .. . . . .2 . 4 1 .5 S 0 4
"N,,,on i c 90 Ba13. -- 17. 5 0. 10 .. .. .. .. .. .. .. .. 2.4 1.6 20 4
"N i,,on 1, 95 Bial. - 17.5 0. 12 ... . .. .... 3.0 2.0 20 4,2 1,22
"N i n, o n 1c 1 0 0 Ba l . - - 2 0 . 0 0 . 2 0 . . . . 5 . 0 . .. . . . . .. . 1 . 3 5 . 0 1 1 4 , 5"N , , ,- m 1 0 5 B a l . - - 2 0 . 0 0 . I s . . . . 5 . 0 . .. . . . . .. . 1 . 2 4 . 7 1 5 4 , 5
1lt.1.r II fak. -- 11.0 0.09 . . 10.0 -.- . . 0.005 -- 3. 1 1.5 19 1,7-9,11-13,16-20, 22
SM-200(71 Bal. 0.25 10 o0. IS .. Iz. 5 1 0. i5 0 05 2 5 9 5,-14,16NASA All~y ra48 B71. " - 0.125 .. .. 4 4 - 8 1 I -- 6 6 Z. S V 11,12'rhoritntBa N,,kcl 1l. - . .. .. .. .. .... .. .. .. 2% ThO2 by 9
'RW- I 9)o0 Bal. -- 10 0. 11 .. .. .. 9 1. 5 -- 0.03 0. 10 1 -- 10. 3 9
U diiiit 700 BaL. -- 18, 5 0. .. .. 5.2 .... .. 0.008 -- 3. S 4 .3 15.0 7,8 ,22
Cobalt-Base Alloys
A F - q 4 1 0 - - R A l . 0 . 1 2 . . . . 5 1 0 l *# . . . . .. 1 5 1 4 , 1 6
Elgiloy Is 16 Bal. 0. 15 2.0 7 20 0.04 He 13H atc ni. i S t ,I &t, v Z . 5 - B S a l. 0 . 2 5 2 . . . 5 . 5 . .. . . . 0 . 0 0 7 , - . . . . . 2 7 1 3 , 14
Alloy 21 maxHaynes Siellite 10.5 -- Bal. 0. S0 .. .. .. 7,5 .. .. .. .. .. .. 25.5 4,13-16,20,
Alloy 1I (X-40) 22Hay-,ci Alloy 25 10 -- Bal. 0. 10 .. .. .. 1S .. .. .. .. ..- .. 20 7,13,15-20,
(L-605) 22J - I •, 7 0 2 8 - - S a l . 0 . 2 -. . . . . . 7 . .. . 4 - - 2 0 1 6S-81b 20 3 Bal. 0. 38 4 4 4a* 20 13SM • (•2 .. .. Bal. 0.85 .. 10 -- 9 0.005 0.20 .. .. 22 14,16
WI 52 .. .. Bal. 0.45 .. .. .. 2 - .. .. .. .. .. 21 14,16X-40 See Haynes Stellite Alloy 31
Iron-Base Alloys
A IS I T y p e 10i4 - 1 0 . 38 a I. - - 0 , 0 6 1 . 5 8 0 . 4 8 . . . .. .. . . . .. 1 7 . 3 7 7ALSI Type 309* 13. 18 Is il. -- 0. 14 1.48 0.69 .. .. .... .. .- 23.04 6,7
AIS1 Type 110* Z5.70 vat. -- 0. 12 1.79 0.43 .. .. .. .. .. .. .. .- 20.03 6,7A1I1 Typc. 330 35.0 gal. -- ).05 1.93 0.80 .. .. .. .. .. .. .. .. 15.43 6,7AIlli T,.pe 347* 10. ;j Bal. -- 0.09 1.22 0.30 -- (0.9)*** .. .. .. .. .. .. 17.82 7I:r oloy*,(
4) 35. 17 Bal. -- 0.04 0.85 0. .2 .. .. .. ... .. .. .. .. 20.20 6,7
Inc1 ioy "T 32.0 Bal. -- 0.04 0. 75 0. 35 .. .. .. .. .. .. 1.0 o0.0 7
19-9 DL 10.0 Bal. -- 0.3I 1.15 0.60 1.3 1.3 0.60"* 0.25 19.0 0. S Cu, 7max.
(1) New Designation by International Nickel Coznpany; Inconel Alloy #00. (7) New Designation by Martin Metals MAR M 200.()21 New Designation by International Nickel Company: Inconel AlleW. (8) Now Designation by Martin Metals MAR. M 302.(3) New Designation by International Nickel Company: Inconol Alto " AActual analysis from Reference 12.(4) New D., ignation by International Nickel Company:.rfrconel AUoyW. *eCb + Ti.(5) New Designation by International Nickel Corrpan•i'* nconal A1l18^41. ***Was not given in analysis.(6) New Destgnat. -n by International Nickel Company: Inconel Alloy 722.
.1
1
11
mi1F
![Page 35: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/35.jpg)
LIST OF DMI TECH7NICL ••PORTS ISSUEDEYenSE METALS INORMATION CET
Battelle Memorial InstituteColumbus, Ohio 43201
t Copies of the technical reports listed below may be obtained from DAIC at no cost by U. S. Governmentagencies, U. S. Government contractors, subcontractors, and/or their suppliers. Others may -purchase copiesof these reports fromi Clearinghouse for Federal Scientific and Technical Information, U. S. Department ofCommerce, Springfield, Virginia 22151. The CFSTI reference numbers (PB or AD prefix numbers) and prices areshown in parentheses. HC refers to Hard Copy price; Mf refers to Microfiche price. Orders to CFSTI shouldrefer to the reference numbers and be prepaid.
Number Title
*150 A Review of Bending Methods for Stainless Steel Tubing, March 2, 1961 (PB 151109, $1.50)151 Environmental and Metallurgical Factors of Stress-Corrosion Cracking in High-Strength Steels,
April 14, 1961 (PB 151110, $0.75)ý152 Binary and Ternary Phase Diagrams of Columbium, Molybdenum, Tantalum, and Tungsten, April 28, 1961
(AD 257739, $3.50)"*153 Physical Metallurgy of Nickel-Base Superalloys, May 5, 1961 (AD 258041, $1.25)
154 Evolution of Ultrahigh-Strength, Hardenable Steels for Solid-Propellant Rocket-Motor Cases, May 25,1961 (AD 257976, $1.25)
155 Oxidation of Tungsten, July 17, 1961 (AD 263598, $3.00)156 Design Information an AM-350 Stainless Steeltfor Aircraft and Missiles, July 28, 1961 (AD 262407,
. $1.50)157 A Summary of the Theory of Fracture in Metals, August 7, 1961 (PB 181081, $1.75)
"*158 Stress-Corrosion Cracking of High-Strength Stainless Steels in Atmospheric Environments, September 15,1961 (AD 266005, $1.25)
159 Gas-Pressure Bonding, September 25, 1961 (AD 265133, $1.25)160 Introduction to Metals for Elevated-Temperature Use, October 27, 1961 (AD 268647, $2.50)161 Status Report No. 1 on Department of Defense Refractory Metals Sheet-Rolling Program, November 2,.
1961 (AD 267077, $1.00)162 Coatings for the Protection of Refractory Metals from Oxidation, November 24, 1961 (AD 271384, $3.50)163 Control of Dimensions in High-Strength Heat-Treated Steel Parts, November 29, 1961 (AD 270045, $1.00)164 Semiaustenitic Precipitation-Hardenable Stainless Steels, December 6, 1961 (AD 274805, $2.75)165 Methods of Evaluating Welded Joints, December 28, 1961 (AD 272088, $2.25)166 The Effect of Nuclear Radiation on Structural Metals, September 15, 1961 (AD 265839, $2.50)
"*167 Summary of the Fifth Meeting of the Refractory Composites Working Group, March 12, 1962 (AD 274804,$2.00)
168 Beryllium for Structural Applications, 1958-1960, May 18, 1962 (AD 278723, $3.50)169 The Effect of Molten Alkali Metals on Containment Metals and Alloys at High Temperatures, May 18,
1962 (AD 278654, $1.50)170 Chemical Vapor Deposition, June 4, 1962 (AD 281887, $2.25)171 The Physical Metallurgy of Cobalt-Base Superalloys, July 6, 1962 (AD 283356, $2.25)172 Background for the Development of Materials'to be Used in High-Strength-Steel Structural Weldmer ts,
July 31, 1962 (AD 284265, $3.00)173 New Developments in Welded Fabrication of Large Solid-Fuel Rocket-Motor Cases, August 6, 1962
(AD 284829, $1.00)174 Electron-Beam Processes, September 15, 1962 (AD 287433, $1.75)175 Summary of the Sixth Meeting of the Refractory Composites Working Group, September 24, 1962 (AD 287029,
$1.75)176 Status Report No. 2 on Department of Defense Refractory Metals Sheet-Rolling Program, October 15, 1962
(AD 288127, $1.25)177 Thermal Radiative Properties of•Selected Materials, November 15, 1962, Volume I (AD 294345, $3.00),
Volume II (AD 294346, $4.00)178 Steels for Large Solid-Propellant Rocket-Motor Cases, November 20, 1962 (AD 292258, $1.00)179 A Guide to the Literature on High-Velocity Metalworking, December 3, 1962 (AD 403493, $3.50)180 Design Considerations in Selecting Materials for Large Solid-Propellant Rocket-Motor Cases, December 10,
1962 (AD 294695, $2.00)181 Joining of Nickel-Base Alloys, December 20, 1962 (AD 296174, $2.00)182 Structural Considerations in Developing Refractory Metal Alloys, January 31, 1963 (AD 419383, $1.00)183 Binary and Ternary Phase Diagrams of Columbium, Molybdenum, Tantalum, ah~d Tungsten (Supplement to
DMIC Report 152), Fcbruary 7, 1963 (AD 407987, $2.75)184 Summary of the Seventh Meeting of the Refractory Composites Working Group, May 30, 1963 (AD 413567,
$1.75)185 The Status and Properties of Titanium Alloys for Thick Plate, June 14, 1963 (AD 421029, $1.50)186 The Effect of Fabrication History and Microstructure on the Mechanical Properties of Refractory
Metals and Alloys, July 10, 1963 (AD 423952, $1.75)187 The Application of Ultrasonic Energy in the Deformation of Metals, August 16, 1963 (AD 423562, $2.25)188 The Engineering Properties of Columbium and Columbium Alloys, September 6, 1963 (AD 426255, $3.50)189 The Engineering Properties of Tantalum and Tantalum Alloys, September 13, 1963 (AD A26344, $2.50)190 The Engineering Properties of Molybdenum and Molybdenum Alloys, September 20, 1963 (AD 426264, $4.00)
* DMIC supply exhausted; copies may be ordered from CFSTI.
![Page 36: OXIDATION OF NICKEL- AND COBALT-BASE … OF NICKEL- AND COBALT-BASE SUPERALLOYS WAY 11 'HARD COPY $. -.ICROFIqIE $. (6-_"o DEFENSE METALS INFORMATION CENTER Battelle Memorial Institute](https://reader031.vdocuments.site/reader031/viewer/2022020315/5a9f110d7f8b9a8e178c48c5/html5/thumbnails/36.jpg)
.64
Number Ti tle
191 The Ehgineering Properties of Tungsten and Tungsten Alloys, September 27, 1963 (AD 425547, $2.75)192 Hot-Cold Working of Steel to Improve Strength, October 11, 1963 (AD 425948, $2.00)193 Tungsten Research and Development Review, October 23, 1963 (AD 425474, $1.50)194 A Discussion of the Physical Metallurgy of the 18 Per Cent Nickel Maraging Steels, November 15, 1963
(AD 430082, $0.75)195 Properties of Coated Refractory Metals, January 10, 1964 (AD 433782, $2.25)196 Hydrogen-Induced, Delayed, Brittle Failures of High-Strength Steels, January'20, 1964 (AD 601116,
$3.00)197 Cracking in High-Strength Steel Weldments - A Critical Review, February 7, 1964 (AD 438432, $4.00)198 The Mechanical Properties of the 18 Per Cent Nickel Maraging Steels, February 24, 1964 (AD 600427,
$2.75)199 The Application of High Pressure in Metal-Deformation Processing - Report of an Informal Symposium
of the Metalworking Process and Equipment Program, March 2, 1964 (AD 437328, $2.00)200 Vacuum Degassing in the Production of Premium-Quality Steels, March 11, 1964 (AD 601823, $4.00)201 U. S. Government Metalworking Processes and Equipment Program, March 18, 1964 (AD 600088, $2.25)202 The Effects of High-Pr, ssure, High-Temperature Hydrogen on Steel, March 26, 1964 (AD 601389, $2.00)203 Explosive Forming of Vatals, May 8, 1964204 The Welding and Brazing of Alloy 718, June 1, 1964205 The Effects of Heat-Treating and Testing Environments on the Properties of Refractory Metals,
August 20, 1964206 An Introduction to Magnesium Alloys, August 26, 1964207 Current Methods of Fracture-Toughness Testing of High-Strength Alloys With Emphasis on Plane Strain,
August 31, 1964208 Metal Deformation Processing, Volume 1, A Survey Conducted as Part of the Metalworking Process
and Equipment Program (MPEP), August 14, 1964209 Second Status Report of the U. S. Government Metalworking Processes and Equipment Program,
November 23, 1964210 Problems !n the Load-Carrying Application of High-Strength Steels, October 26-28, 1964211 Premium-Quality Aluminum Castings, January 4, 1965212 Department of Defense Refractory Metals Sheet Rolling Program, Status Report No. 3, January 26, 1965213 Metal Removal by Electrochemical Methods and Its Effects on Mechanical Properties of Metals,
January 7, 1965