improved nanoindentation techniques for wood...

48
Improved Nanoindentation Techniques for Wood Research Joseph Jakes USFS Forest Products Laboratory University of Wisconsin-Madison Materials Science Program Advisor at UW: Don Stone Advisors at FPL: Chuck Frihart and Jim Beecher

Upload: others

Post on 22-Aug-2020

2 views

Category:

Documents


0 download

TRANSCRIPT

Page 1: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Improved Nanoindentation

Techniques for Wood Research

Joseph JakesUSFS Forest Products Laboratory

University of Wisconsin-Madison

Materials Science Program

Advisor at UW: Don Stone

Advisors at FPL: Chuck Frihart and Jim Beecher

Page 3: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Preview

Indents in CCML Indents in SCWL

2 µm

2 µm

Specimen violates assumptions of standard analyses:

-Structural heterogeneities present

-Specimen-scale flexing

Properties are time- and pressure-dependent

Heterophase

Interfaces

Free EdgesHeterophase

Interfaces

Page 4: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Outline

• Specimen preparation

• Standard nanoindentation analysis

• Method to account for structural heterogeneities and

specimen-scale flexing

– Introduce a structural compliance (Cs) into the standard

analysis

– Cs behaves similar to machine compliance (Cm)

– Cs can be experimentally measured with the same

correlation (SYS correlation) used to calculate Cm

• Methods to measure rate-dependent hardness

• Ethylene glycol modified wood

Page 6: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Preparing Wood Specimens for

Nanoindentation• Current literature embed wood specimens in epoxy

– Diffusion of epoxy components may be altering cell wall

• Developed microtoming technique– Create pyramid with disposable microtome blades in sledge

microtome

– Cut off apex with diamond knife in rotary ultramicrotome

C

A

C

B

A

5 µm

Diamond knife

cut

10 mm

Latewood

Page 8: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Ideal Nanoindentation Experiment

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

Depth

Lo

adInfinite half-space

Oliver and Pharr (1992) J. Mater. Res. 7(6) pp. 1564.

Page 9: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Standard Nanoindentation Analysis

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

Depth

Lo

adInfinite half-space

chA

PH max

S

Phhc

maxmax

S

1

Pmax

hc

hc

hmax

Page 10: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Standard Nanoindentation Analysis

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

Depth

Lo

adInfinite half-space

S

1

Pmax

hc

hc

c

effhA

SE

d

d

s

s

eff EEE

22 1111

chA

PH max

Page 11: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Ideal Nanoindentation Experiment

Infinite half-space

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

Depth

Lo

ad

Page 12: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Real Nanoindentation Experiment

Infinite half-space

Cm

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

Depth

Lo

ad

cmtcpc

effhACChAChA

SE

11

0 50 100 150 200 250 300

Depth, h (nm)

0

200

400

600

800

1000

Lo

ad.

L(

N)

Load-depth trace

not corrected for

Cm

Page 14: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Nanoindentation of Wood

Cellular Structure

Page 15: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Silicon Bridge to Validate

Specimen-scale flexing

#1 #2 #3 #4

Top view

Jakes et al. (2008) J. Mater. Res. 23(4) pp. 1113.

Side view

Page 16: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Silicon Bridge to Validate

Specimen-scale flexing

#1 #2 #3 #4

Modulus (Es)

underestimated when

indents placed over

unsupported region

Standard Analysis

0 2 4 6 8 10

Lmax (mN)

0

50

100

150

200

Es

(GP

a)

#1

#2

#3

#4

Jakes et al. (2008) J. Mater. Res. 23(4) pp. 1113.

P

Page 17: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

#1 #2 #3 #4

Hypothesized additional

compliance over unsupported

region behaves similar to Cm

(independent of load)

Silicon Bridge to Validate

Specimen-scale flexing

PCPCPC pmt

eff

mtE

HPCPC

eff

ppE

H

A

PACPC

SYS Correlation

Plot Ct√P vs. √PStone et al. (1991) J. Vac. Sci.

Technol. A 9(4) pp. 2543-2547

Page 18: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

#1 #2 #3 #4

Hypothesized additional

compliance over unsupported

region behaves similar to Cm

(independent of load)

0.00 0.03 0.06 0.09 0.12

L (N1/2

)

0.0

0.5

1.0

1.5

2.0

2.5

3.0

Ct

L(

m/N

1/2

)

SYS Correlation

#4

#3

#2

#1

Cm = 21 µm/N > Cm,meas

Cm = 3 µm/N = Cm,meas

Silicon Bridge to Validate

Specimen-scale flexing

eff

mtE

HPCPC

Jakes et al. (2008) J. Mater.

Res. 23(4) pp. 1113.

P

P

Page 19: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

eff

smtE

HPCCPC

#1 #2 #3 #4

Hypothesized additional

compliance over unsupported

region behaves similar to Cm

(independent of load)

SYS Correlation

Silicon Bridge to Validate

Specimen-scale flexing

Jakes et al. (2008) J. Mater.

Res. 23(4) pp. 1113.

0.00 0.03 0.06 0.09 0.12

L (N1/2

)

0.0

0.5

1.0

1.5

2.0

2.5

3.0

Ct

L(

m/N

1/2

)

#4

#3

#2

#1

Cm = 21 µm/N > Cm,meas

Cm = 3 µm/N = Cm,meas

P

P

Page 20: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

0 2 4 6 8 10

Lmax (mN)

0

50

100

150

200

Es

(GP

a)

#1 #2 #3 #4

Corrected Analysis

#1

#2

#3

#4

Es = 162 3 GPa

H = 12.5 ± 0.3 GPa

Average after accounting for Cs

smtmeas

effCCCA

E1

meas

max

A

PH

Silicon Bridge to Validate

Specimen-scale flexing

P

Page 21: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Nanoindentation of Wood

Cellular Structure

No method exists to experimentally account for

effect of free edge

Edge

Page 22: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Fused Silica to Validate Edge

Effects

5 µm

Edge of Specimen

0.5 µm

Edge of Specimen

Standard Analysis

Modulus (Es) underestimated

when indents approach edge

0 2 4 6 8 10 12 14

Distance from edge, d ( m)

40

50

60

70

80

Mo

du

lus,

Es

(GP

a)

0

2

4

6

8

10

12

14

Har

dn

ess,

H(G

Pa)

Page 23: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

5 µm

Edge of Specimen

0.5 µm

Edge of Specimen

Multiple load indent

Need compliance

as function of load

Fused Silica to Validate Edge

Effects

0.00 0.05 0.10 0.15 0.20 0.25 0.30 0.35

Depth. h ( m)

0

2

4

6

8

10

Lo

ad,

L(m

N)

Depth, h

Lo

ad, P

eff

smtE

HPCCPC

Page 24: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

5 µm

Edge of Specimen

0.5 µm

Edge of Specimen

SYS Correlation

0.00 0.03 0.06 0.09 0.12

L (N1/2

)

1.2

1.4

1.6

1.8

2.0

2.2

Ct

L(

m/N

1/2

)

Edge effects contribute

to Cs and is independent

of load

Increasing distance

from edge

Fused Silica to Validate Edge

Effects

eff

smtE

HPCCPC

P

P

Page 25: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

5 µm

Edge of Specimen

0.5 µm

Edge of Specimen

eff

smtE

HLCCLC

Increasing distance

from edge

Fused Silica to Validate Edge

Effects

0 2 4 6 8 10 12 14

d ( m)

40

50

60

70

80

Mo

du

lus,

Es

(GP

a)

0

2

4

6

8

10

12

14

Har

dn

ess,

H(G

Pa)

Corrected AnalysisStandard Analysis Neglecting Cs

Standard Analysis Accounting for Cs

Es = 72.1 0.5 GPa

H = 11.1 ± 0.1 GPa

Accounting for Cs

Page 26: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Nanoindentation of Wood

0.0 0.2 0.4 0.6 0.8 1.0

Lmax (mN)

12

14

16

18

20

22

Mo

du

lus,

Es

(GP

a)

0

100

200

300

400

500

600

Har

dn

ess,

H(M

Pa)

Corrected AnalysisStandard Analysis

5 µm

Empty Lumen

P

Page 27: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Cs from Heterophase Interface

(Substrate-Adhesive)

Will the same method work for a

heterophase interface?

Adhesive, Es,adh Substrate, Es,sub

Es,sub > Es,adh

Behave similar to

free edge

Page 28: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Will the same method work for a

heterophase interface?

Adhesive, Es,adh

Constraining effect

from stiffer phase?Es,sub > Es,adh

Substrate, Es,sub

Cs from Heterophase Interface

(Substrate-Adhesive)

Page 30: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Nanoindentation of Polypropylene-

Wood Composite

SYS Correlation2 µm

Positive Cs suggests

this is a crack

0.000 0.010 0.020 0.030

L (N1/2

)

2.0

2.5

3.0

3.5

4.0

4.5

5.0

Ct

L(

m/N

1/2

)

Cs = 4 µm/N

Cs = -21 µm/N

eff

smtE

HPCCPC

P

P

Page 31: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Nanoindentation of Polypropylene-

Wood Composite

Corrected analysis2 µm

0.0

1.0

2.0

3.0

Es

(GP

a)

Filled symbols are the

corrected analysis

Our methods are also capable of accounting for

heterophase interfaces and detecting cracks

Page 32: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

External Compliances in Real

Nanoindentation Experiments

• Machine Compliance (Cm)– Property of nanoindenter

• Constant for every indent performed

– Standard methods established to account for Cm

• Structural Compliance (Cs)– Property of specimen and location of indent

• Specimen-scale flexing

• Heterophase interphases

– Need to use methods we developed to measure Cs

• Jakes et al. (2008) J. Mater. Res. 23(4) pp. 1113.

• Jakes et al. (2009) J. Mater. Res. 24(3) pp. 1016.

SYS Correlation:eff

smtE

HPCCPC

Page 34: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

PMMA Rate-dependence Hardness

0.1 s load to 10mN

50 s hold at 10 mN

0.1 s unload

Need method to determine decrease in

hardness with increasing creep time

Page 35: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

50 s10 s1 s

0.5 s

0.2 s

0.1 s

0.05 s

0.01 s

Varying hold times

0.1 s load to 10mN

0.01 to 50 s hold at 10 mN

0.1 s unload

Measure areas to determine decrease in

hardness with increasing creep time

PMMA Rate-dependence Hardness

from Direct Observation

Page 36: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

0.5 µm

50 s

hold

0.01 s

hold

0.5 µm

0.01 s hold

0.05 s hold

0.10 s hold

0.20 s hold

0.50 s hold

1.00 s hold

10.0 s hold

50.0 s hold

PMMA Rate-dependence Hardness

from Direct Observation

Puthoff et al. (2009) J. Mater. Res. 24(3) pp. 1279.

Page 37: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

A

PH

PMMA Rate-dependence Hardness from

Instantaneous Hardness Based on Depth

Puthoff et al. (2009) J. Mater. Res. 24(3) pp. 1279.

Page 38: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

10-4

10-3

10-2

10-1

100

101

102

d H/dt (s-1

)

2.5

2.6

2.7

2.8

2.9

3.0

3.1

log(H

)(M

Pa)

dt

AdH

ln

H

PMMA Rate-dependence Hardness from

Instantaneous Hardness Based on Depth

Puthoff et al. (2009) J. Mater. Res. 24(3) pp. 1279.

Page 40: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Experimental Procedure

• Loblolly pine (Pinus taeda)– S2 cell wall lamina (SCWL) and compound corner middle lamella

(CCML) probed

• Untreated specimen tested

• Soaked untreated specimen in ethylene glycol for 3 days to modify it

• Treated specimen tested

• Indentation performed with Hysitron Triboindenter– Multiload indents with 50 s hold segment for creep

– RH controlled at ~35% with glycerol-water bath

• Structure compliance measured

• Rate-dependent hardness determined using mathematical model

Page 41: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Unmodified Wood

2 µm

21 1.2 mN indents

Es = 21 3 GPa

H = 380 ± 20 MPa

6 0.8 mN indents

Es = 6 1 GPa

H = 340 ± 20 MPa

2 µm

CCML SCWL

Page 44: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Ethylene Glycol Modified Wood

2 µm

18 0.4 mN indents

Es = 6 4 GPa

H = 80 ± 10 MPa

5 0.2 mN indents

Es = 2 1 GPa

H = 80 ± 40 MPa

2 µm

No residual indent! Used area based

on contact depth for calculations

CCML SCWL

Page 45: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

10-4

10-3

10-2

10-1

100

101

102

H (s-1

)

102

103

Har

dn

ess

(MP

a)

Unmodified SCWLUnmodified CCMLEG-modified SCWLEG-modified CCML

Rate-dependence of Hardness

Jakes et al. (2008) Mater. Res. Soc. Proc. paper # 1132-Z07-21.

Page 46: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Ethylene Glycol Modified Wood

• Ethylene glycol entered and plasticizes both SCWL and CCML– Residual indents recovered

– SCWL and CCML swelled

– Es and H decreased

• Ethylene glycol affects H of SCWL and CCML differently at high strain rates

• Nanoindentation provides mechanical characterization of micron-size domains in wood– Accounts for structural heterogeneities and specimen-scale flexing

– Measure rate-dependent hardness over 4 decades strain rate

• Nanoindentation one tool to investigate modified wood– Chemical analyses

– Microscopy

– Bulk wood characterization

Page 47: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Conclusions

• Developed methods to account for specimen-scale flexing and structural heterogeneities– Cs

– Independent of load

– Measured with SYS correlation

• Rate-dependent hardness– Measured over 4-5 decades of strain rate

• Direct observation or mathematical model

• Ethylene glycol modified wood– Ethylene glycol entered and plasticized both the SCWL and CCML

Page 48: Improved Nanoindentation Techniques for Wood Researchcost-fp0802.tuwien.ac.at/fileadmin/mediapool-cost/Bilder/WS/... · 0 50 100 150 200 250 300 Depth, h (nm) 0 200 400 600 800 1000

Thank you!

Questions?

2 µm