fiber reinforced superalloys - nasa · pdf file · 2013-08-30fiber reinforced...
TRANSCRIPT
![Page 1: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/1.jpg)
NASA Technical Memorandum 89865
Fiber Reinforced Superalloys
Donald W. Petrasek and Robert A. Signorelli Lewis Research Center Cleveland, Ohio
and
Thomas Caulfield and John K . Tien Coliirrzbia University New York, New York
(EASA-3W-89865) € I B E I i R E I N E C G C E D id0 7-2 28 I 1 SOPEBALLCYS (HAS&) 62 p A v a i l : NTIS HC 404/ClP A01 C S C L l l D
Ulaclas g/i?4 0074224
April 1987
https://ntrs.nasa.gov/search.jsp?R=19870013378 2018-05-21T18:04:17+00:00Z
![Page 2: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/2.jpg)
F I B E R REINfORCED SUPERALLOYS
Donald W. Pet rasek and Robert A. Signore111 N a t i o n a l Ae ronau t i cs and Space A d m i n i s t r a t i o n
Lewis Research Center Cleveland. Ohio 44135
and
Thomas C a u l f i e l d and John K. T i e n Columbia U n i v e r s i t y
New York, New York 10027
SUMMARY
Improved performance o f heat engines 1 s l a r g e l y dependent upon maximum
c y c l e temperatures. Tungsten f i b e r r e l n f o r c e d s u p e r a l l o y s (TFRS) a r e t h e
f i r s t o f a f a m i l y of h i g h temperature composites t h a t o f f e r t h e p o t e n t i a l f o r
s i g n i f i c a n t l y r a i s i n g h o t component ope ra t i ng temperatures and thus l e a d i n g t o
improved h e a t engine performance. Thls s t a t u s r e v i e w o f TFRS research empha-
s i z e s t h e p r o m i s l n g p r o p e r t y d a t a developed t o da te , t h e s t a t u s o f TFRS com-
p o s i t e a i r f o i l f a b r i c a t i o n technology, and t h e areas r e q u i r i n g more a t t e n t i o n
t o assu re t h e i r a p p l i c a b i l i t y t o h o t s e c t i o n components o f a i r c r a f t g a s - t u r b i n e
engines .
![Page 3: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/3.jpg)
The need for improved materials at elevated temperatures has stimulated
research in many areas including efforts to develop fiber reinforced superalloy
matrix composltes. A number of fibers have been studled for such use including
submicron diameter ceramic whiskers, continuous length ceramic filaments, boron
filaments, carbon filaments, and refractory metal alloy wires. Attainment of
high temperature strength with superalloy matrlx composites has been successful
using refractory metal alloy wires, but the use of ceramic whiskers, continuous
length ceramic filaments, boron filaments or carbon filaments as the reinforc-
ing fiber has been unsuccessful to date.
The theoretical speclfic strength potentlal o f refractory alloy fiber
reinforced superalloys is less than that of ceramic fiber reinforced super-
alloys. However, the more ductile metal fiber systems are more tolerant of
fiber-matrix reactions and thermal expanslon mismatches. Also, the superalloy
matrices can protect high strength refractory metal fibers from environmental
attack. In laboratory tests, refractory fiber relnforced superalloy composites
have demonstrated stress-rupture strengths signtficantly above those of the
strongest superalloys. Tungsten fiber reinforced superalloy composites, In
particular, are potentially useful as high temperature (1000 to 1200 "C (1830
to 2190 O F ) materials because they have many deslrable properties such as good
stress-rupture and creep resistance, oxidation resistance, ductlllty, lmpact
damage resistance, thermal conductivity and microstructural stability. The
potential of tungsten fiber relnforced superalloys (TFRS) has been recognized
and has stimulated research to develop this material for use in heat engines.
The object o f this paper is to revlew the development of fiber reinforced
superalloys. First refractory metal fiber and matrlx alloy development wlll
be reviewed. This will be followed by a discussion of fabrication techniques
2
![Page 4: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/4.jpg)
f o r TFRS and p r o p e r t y r e s u l t s o f importance f o r t h e i r use a t h i g h temperatures.
Component f a b r i c a t i o n and f a b r i c a t i o n c o s t d a t a f o r a s p e c i f i c TFRS system w i l l
t hen be d iscussed i n t h e f i n a l s e c t i o n .
I. FIBER DEVELOPMENT
R e f r a c t o r y me ta l w i r e s have received a g r e a t dea l o f a t t e n t i o n as f i b e r
r e i n f o r c e m e n t m a t e r i a l s f o r h i g h use temperature composites i n s p i t e o f t h e i r
poor o x i d a t i o n r e s i s t a n c e and h i g h dens i t y . When used t o r e i n f o r c e a d u c t i l e
and o x i d a t i o n r e s i s t a n t m a t r i x , t hey are p r o t e c t e d f rom o x i d a t i o n and t h e i r
s p e c i f i c s t r e n g t h I s much h i g h e r t h a n t h a t o f s u p e r a l l o y s a t e l e v a t e d tempera-
t u r e s . The m a j o r i t y o f t h e s t u d i e s conducted on r e f r a c t o r y w i r e / s u p e r a l l o y
composites have used t u n g s t e n o r molybdenum w i r e , a v a i l a b l e as lamp f i l a m e n t o r
thermocouple w i r e , as t h e r e i n f o r c e m e n t m a t e r i a l . These r e f r a c t o r y a l l o y s were
n o t designed f o r use i n composi tes no r f o r optimum mechanical p r o p e r t i e s i n t h e
temperature range o f i n t e r e s t f o r h e a t engine a p p l i c a t i o n , 1000 t o 1200 O C
(1830 t o 2190 OF). Lamp-f i lament w i r e such as 218CS tungs ten was most ex ten -
s i v e l y used i n e a r l y s t u d i e s . The s t r e s s - r u p t u r e p r o p e r t i e s o f 218CS t u n g s t e n
w i r e were s u p e r i o r t o those o f r o d and bu lk forms o f t ungs ten and showed prom-
i s e f o r use as r e i n f o r c e m e n t o f supera l l oys . The need f o r s t r o n g e r w i r e was
recognized, and h l g h s t r e n g t h tungsten, tanta lum, molybdenum, and n i o b i u m
a l l o y s f o r which r o d and/or sheet
developed were l n c l u d e d i n a w i r e
1970; K ing, 1972; Petrasek, 1972;
chemical composi t ions o f t hese a1
f a b r i c a t i o n procedures had a l r e a d y been
f a b r i c a t i o n and t e s t program, (Amra e t a l . ,
and Petrasek and S i g n o r e l l i , 1969). The
oy are g i v e n i n Table I . The above approach
p rec luded development o f new a l l o y s s p e c i f i c a l l y designed f o r s t r e n g t h a t t h e
i n tended composl te use temperatures. The s t r e s s - r u p t u r e and t e n s i l e p r o p e r t i e s
determined f o r t h e w i r e s developed a r e summarized i n Table I 1 and a r e compared
w i t h commer l ca l l y a v a i l a b l e w i r e (218CS, W-1 Tho2 and W-3Re).
E x c e l l e n t p rog ress was made i n p r o v i d i n g w i r e s w i t h i nc reased s t r e n g t h
compared t o t h e s t r o n g e s t w i r e s wh ich were p r e v i o u s l y a v a i l a b l e . The u l t i m a t e
3
![Page 5: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/5.jpg)
t e n s i l e s t reng ths o b t a i n e d f o r t h e w i r e s a t 1093 and 1204 " C (2000 and 2200 O F )
a r e p l o t t e d i n F i g . 1 . Tungsten a l l o y w i r e s were f a b r i c a t e d hav ing t e n s i l e
s t r e n g t h s 2-1/2 t imes t h a t o b t a i n e d f o r 218CS tungs ten w i r e . The s t r o n g e s t
w i r e f a b r i c a t e d , W-Re-Hf-C, had a t e n s i l e s t r e n g t h o f 2165 MN/m (314 k s l ) a t
1093 "C (2000 O F ) which i s more than 6 t imes a s s t r o n g as t h e s t r o n g e s t n l c k e l
o r c o b a l t base s u p e r a l l o y . The u l t i m a t e t e n s i l e s t r e n g t h va lues ob ta ined f o r
t h e tungsten a l l o y w i r e s were much h i g h e r t h a n those ob ta ined f o r molybdenum,
t a n t a l u m or n i o b i u m a l l o y w i r e . When d e n s i t y i s t aken i n t o account, t h e tung-
s t e n a l l o y w i r e s show a decrease i n advantage compared t o tanta lum, n i o b i u m o r
molybdenum w i r e , F i g . 2. However, t h e h i g h s t r e n g t h tungs ten a l l o y w i r e s as
w e l l as molybdenum w i r e s o f f e r t h e most promise.
2
The e leva ted s t r e s s - r u p t u r e s t r e n g t h o f r e i n f o r c i n g w i r e i s more s i g n i f i -
c a n t t han the t e n s i l e s t r e n g t h , s i n c e t h e i n tended use o f t h e m a t e r i a l i s f o r
l o n g t i m e a p p l i c a t i o n s . The 100 h r r u p t u r e s t r e n g t h a t 1093 and 1204 O C (2000
and 2200 O F ) i s p l o t t e d f o r t h e v a r i o u s w i r e m a t e r i a l s and compared t o super-
a l l o y s i n Flg. 3 . The r u p t u r e s t r e n g t h o f t u n g s t e n a l l o y f i b e r s was inc reased
by a f a c t o r o f 3 a t 1093 "C (2000 O F ) f r o m about 434 MN/m ( 6 3 k s i ) f o r 218CS
tungs ten t o 1413 MN/m (205 k s i ) f o r W-Re-Hf-C w i r e . The tungs ten a l l o y w i r e
was super io r i n s t r e s s - r u p t u r e s t r e n g t h t o t h e o t h e r r e f r a c t o r y w i r e m a t e r i a l s
w i t h t h e excep t ion o f a t a n t a l u m a l l o y , ASTAR 811C, which was s t r o n g e r t h a n
most o f t he tungs ten a l l o y m a t e r i a l s a t 1093 O C (2000 O F ) . The s t r o n g e s t
t ungs ten a l l o y w i r e , W-Re-Hf-C, was over 16 t imes as s t r o n g as s u p e r a l l o y s a t
1093 "C (2000 O F ) . The 100 h r r u p t u r e s t r e n g t h t o d e n s i t y va lues f o r r e f r a c -
t o r y me ta l s w i r e s and s u p e r a l l o y s a r e p l o t t e d i n F i g . 4. Agaln t h e s t r o n g e r
tungs ten w i r e m a t e r i a l s a r e s u p e r i o r t o t h e o t h e r r e f r a c t o r y me ta l w i r e s . When
d e n s i t y i s taken i n t o account, t h e s t r o n g e s t t ungs ten w i r e m a t e r i a l , W-Re-Hf-C,
2
2
i s more than 7 t imes as s t r o n g as t h e s t r o n g e s t s u p e r a l l o y s a t 1093 "C (2000 O F ) .
4
![Page 6: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/6.jpg)
The p r o c e s s i n g schedules used t o f a b r i c a t e t h e newer h i g h s t r e n g t h w i r e s
were n o t o p t i m i z e d t o p r o v i d e maximum s t r e n g t h a t 1093 and 1204 " C (2000 and
2200 O F ) . Much more work i s needed t o maximize t h e i r p r o p e r t i e s . Cons ide rab le
o p p o r t u n i t y e x i s t s t o develop w i r e process ing schedules t a i l o r e d f o r f i b e r -
m a t r i x composi te use. The even tua l a p p l i c a t i o n o f TFRS composites w i l l j u s t i f y
t h e added e f f o r t t o f u r t h e r improve w i r e p r o p e r t i e s .
11. MATRIX-ALLOY DEVELOPMENT
The m a t r i x i s t h e exposed component o f f i b e r r e i n f o r c e d composi tes and
t h e r e f o r e must be a b l e t o w i t h s t a n d h i g h temperatures and an environment which
can r e s u l t i n c a t a s t r o p h i c o x i d a t i o n and h o t c o r r o s i o n . The p r i m a r y f u n c t i o n
o f t h e m a t r i x I s t o b i n d t h e f i b e r s i n t o a u s e f u l body and t o p r o t e c t t h e
f i b e r s f r o m o x i d a t i o n and h o t c o r r o s i o n . The m a t r i x must be r e l a t i v e l y d u c t i l e
compared t o t h e f i b e r s t o f a c i l i t a t e load t r a n s f e r f r o m t h e m a t r i x t o t h e
f i b e r . I t a l s o must be capable o f evenly r e d i s t r i b u t i n g l o c a l s t r e s s concen-
t r a t i o n s and r e s i s t i n g a b r a s i o n and impact damage f r o m f o r e i g n o b j e c t s . The
m a t r i x and r e i n f o r c i n g f i b e r must be able t o c o - e x i s t w i t h o u t m u t u a l l y induced
d e g r a d a t i o n t h a t can r e s u l t f r o m chemical i n t e r a c t i o n s t h a t can reduce b o t h t h e
f i b e r and m a t r i x p r o p e r t i e s .
t i o n o f m a t r i x compos i t i on i s t h e a b i l i t y o f t h e m a t r i x t o f o r m a good bond
w i t h t h e f i b e r w i t h o u t excess i ve r e a c t i o n o c c u r i n g which c o u l d degrade t h e
f i b e r s p r o p e r t i e s .
The most impor tan t f a c t o r i n t h e i n i t i a l s e l e c -
For h i g h tempera tu re use, n icke l -base, cobal t -base and i ron -base super-
a l l o y s a r e p r e f e r r e d as t h e m a t r i c e s f o r r e f r a c t o r y me ta l f i b e r composi tes
because t h e y have demonstrated s t r e n g t h and d u c t i l i t y a t e l e v a t e d temperatures,
as w e l l as good o x i d a t i o n and h o t c o r r o s i o n r e s i s t a n c e .
A l a r g e p r o p o r t i o n o f t h e research e f f o r t conducted on r e f r a c t o r y f l b e r
composi tes has been on f i b e r - m a t r i x c o m p a t i b i l i t y . E f f o r t s have focused on
deve lop ing s t r u c t u r a l l y s t a b l e composites by choosing a m a t r i x compos i t i on
5
![Page 7: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/7.jpg)
which does not severely degrade the properties of the reinforcing fiber. One
of the first systematic examinations to determine the effect of alloying reac-
tions on the strength and microstructure of refractory metal fiber composites
was reported by Petrasek and Weeton (1963) where copper-based binary alloys
were used as a matrix for tungsten-fiber composites. The effects of alloying
element additions to copper on the strength and microstructure o f tungsten
fiber composites were compared with mutally insoluble pure copper matrlx com-
posites exposed under the same conditions. The alloying elements studied were
aluminum, chromium, cobalt, niobium, nickel, zirconium and titanium. Data
obtained for solute elements in this system can be related to the expected
behavior o f these same elements in superalloys. These effects served as the
basis for modifying superalloy matrix composition to control fiber-matrix
reactlon. Three types of fiber-matrix reaction were found to occur: ( 1 )
diffusion-penetration reaction accompanied by a recrystallization of a periph-
eral zone of the tungsten fiber; (2) precipitation of a second phase with no
accompanying recrystallization; (3) a solid solution reaction with no accompany-
ing recrystallization In the fiber. Peripheral recrystallization was caused
by diffusion of cobalt, aluminum, or nickel into the tungsten wire. Compound
formation occurred with titanium and zirconium. Chromium and niobium In copper
formed a solid solution with tungsten with no accompanying recrystallization of
the tungsten fiber. The greatest damage to composite properties occurred with
the penetration-recrystalllzation reactlon while the two-phase and solld solu-
tion reactions caused relatively little damage. Recrystallization of tungsten
fibers in a Cu-10 percent Ni matrlx i s shown in Fig. 5.
Similar results were later found in a number of studies conducted on
nickel-induced recrystallization of tungsten fibers, (Gruenling and Hofer,
1974; Hoffman et al., 1974; and Montelbano et al., 1968). Recrystallization
could be induced at low temperature by the presence of solid nickel on the
6
![Page 8: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/8.jpg)
surface of the tungsten wire. Once initiated, nickel-induced recrystalli-
zation required a continued source of nickel for propagation of the recrystal-
lization front. Work reported by Montelbano et al. (1968) found that palladium,
aluminum, manganese, platinum and iron also greatly lowered the recrystalliza-
tion temperature o f tungsten.
Based on such findings, superalloy matrix compositions were developed that
caused limited reaction with the fiber and minimal fiber-property loss (Petrasek
et al., 1968). These superalloys contained high welght percentages of refrac-
tory metals to reduce diffusion penetration of nickel into tungsten. Additions
of Ti and A1 to the matrix were also made to form intermetallic compounds which
would further reduce the diffusion of nickel into tungsten. A typical matrix
alloy that was developed was Ni-25W-15Cr-2Al-Ti. The fiber stress to cause
rupture in 100 hr at 1090 "C (2000 O F ) was reduced only 10 percent in compos-
ites using this alloy as a matrix compared to the equivalent fiber rupture
strength tested in a vacuum outside a composite.
The problem of obtaining structure-stable composite materials from the
nickel-tungsten and nickel-molybdenum systems were further examined by Karp nos
et al. (1972). The results obtained showed that in reinforced metal compos t e
materials, in which the matrix and fiber form restricted solid solutions in the
absence of intermetallic compounds, minlmal fiber dissolution can be achieved
by alloying the matrix with the fiber metal up to a concentration that is close
to the solubility limlt. However, when the matrix and the fiber react to form
intermetallic compounds, matrix saturation i s not effective in controlling
fiber attack by dlssolution.
The effect of the composition of nickel, cobalt and iron-base alloys on
the structural stability of composite materials reinforced with tungsten fibers
was determined by several investlgators (Brentnall, 1976; Klypin et al., 1977;
1
![Page 9: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/9.jpg)
and M l r o t v o r s k l i and O l ' s h e v s k i i , 1976, 1978, and 1979) . The r a t e of I n t e r -
a c t i o n between t h e f i b e r and t h e m a t r i x was determined f rom t h e e x t e n t o f
r e c r y s t a l l i z a t i o n o f t h e f i b e r ; t h e f o r m a t i o n o f i n t e r m e d i a t e phases a t t h e
i n t e r f a c e ; the s o l u t i o n o f t h e f i b e r i n t h e m a t r i x ; and t h e f o r m a t i o n o f d i f -
f u s i o n a l p o r o s i t y .
F i b e r r e i n f o r c e d b i n a r y and mult icomponent cobal t -base a l l o y s were found
t o have a s t rong p r o p e n s i t y t o i n t e r m e t a l l i c compound f o r m a t i o n a t t h e m a t r i x
f i b e r i n t e r f a c e . Complex a l l o y i n g a d d l t i o n s t o i ron-base a l l o y s were found t o
o f f e r a means o f suppress ing f i b e r r e c r y s t a l l i z a t i o n and t h e f o r m a t i o n o f i n t e r -
m e t a l l i c compounds a t t h e i n t e r f a c e between t h e tungs ten f i b e r s and t h e i r o n -
base m a t r i x . R e s u l t s o f t h e r e a c t i o n o f t ungs ten f i b e r s w i t h b i n a r y a l l o y s o f
i r o n , n i c k e l , and c o b a l t annealed a t 1200 and 1300 " C (2190 and 2370 O F ) f o r
1 h r ( M i r o t v o r s k i i and O l ' s h e v s k l i , 1979) a r e summarized i n Table 111. Shown
i n Table 111 a r e t h e number o f composi t ions i n v e s t i g a t e d f o r each m a t r i x system
and t h e r e l a t i v e number o f cases, based on a percentage, t h a t r e s u l t s i n t h e
f o l l o w i n g r e a c t i o n s w i t h t h e tungs ten f i b e r ; r e c r y s t a l l i z a t i o n ; f o r m a t i o n o f an
i n t e r m e t a l l l c compound; a d i f f u s i o n a l p e n e t r a t i o n i n t o t h e f i b e r ; and no d e t e c t -
a b l e r e c r y s t a l l i z a t i o n o r r e a c t i o n w i t h t h e f i b e r .
found t o be l e a s t r e a c t i v e i n i r on -base a l l o y m a t r i c e s . A number o f m a t r l x
composi t ions have been i d e n t i f i e d , p a r t i c u l a r l y f o r i ron-base a l l o y s , i n which
no d e t e c t a b l e r e a c t l o n occu rs w i t h tungs ten f i b e r s a f t e r s h o r t t i m e exposures
a t temperatures up t o 1200 "C (2190 O F ) .
The tungs ten f i b e r s were
Recent s t u d i e s by C a u l f i e l d (1986) and C a u l f i e l d e t a l . (1985) have cen te red
on m i n i m i z i n g r e a c t i o n zone g rowth i n TFRS composi tes f o r l ong - te rm a p p l i c a -
t i o n s ( > l o h r ) i n t h e tempera tu re range of 1050 t o 1200 O C (1920 t o 2190 O F )
by m o d i f y i n g m a t r i x a l l o y c h e m i s t r l e s . The k i n e t i c s and r a t e controlling
process f o r r e a c t l o n zone g rowth were a s c e r t a i n e d by d i r e c t a p p l i c a t i o n o f t h e
moving boundary equa t ions t o r e a c t i o n zone growth. T h e i r r e s u l t s show t h a t
8
![Page 10: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/10.jpg)
reaction zone growth i s rate controlled by interdiffusion across the reaction
zone and that the interdiffusion coefficlent of the reaction zone phase, and
thus the kinetics for reaction growth, are matrix chemistry dependent.
Table I V i s a list of the parabolic rate constants, K ( T ) , for reaction rz zone growth for various W-fiberhetal matrix composites. The tabulated data
reveal that the kinetics of reaction zone growth substantially decrease with
simultaneous increases in the matrix Ni content and decreases in the matrix Fe
and Co content. Since the Waspaloy matrix TFRS composite exhibited the slowest
reaction zone kinetics, a cobalt-free modlfied Waspaloy matrix alloy was inves-
tigated. The results are unpublished to date; however, preliminary analysis of
the Co-free modified Waspaloy composite reveals that reaction zone kinetics are
at least three times slower than those exhibited by the Waspaloy matrix/W-fiber
composite ( T . Caulfield, A.B. Rodriguez, and J . K . Tien, present study at
(Columbia University, New York, 1987).
Most of the matrix compositions investigated that resulted in minimum
reaction with the fibers Involved the formation of intermetallic compounds
which served to reduce interdiffusion. Thus, intermetallics might be sought as
a natural occurring dlffuslon barrier. Use of a suitable protectlve barrier
between the fiber and matrix offers the possibility of a wlder range of com-
position selection for composites for hlgh temperature application. However,
the introduction of a second interface and a deposited coating, whose possible
breakdown In service at high temperatures would cause a catastrophic decrease
in strength, i s not an attractive alternative to aircraft engine manufacturers
and operators (Morris and Burwood-Smith, 1971). Although diffusion barrier
coatings on reinforcing wlre are a potentially effective way to achieve control
of fiber-matrix interaction, techniques attempted to date have not resulted in
reproducible, successful barrier coatings for refractory alloy wire (Signorelli,
1972). Optimism continues, however, that such natural or deposited coatings
9
![Page 11: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/11.jpg)
are possible and wlll offer increases in both strength and use temperature.
Trade-offs in compound composition and ductility offer a fruitful area for
continued studies.
111. COMPOSITE FABRICATION
The consolidation of matrix and fibers into a composite material with
useful properties is one of the most difficult tasks in developing refractory-
wire-reinforced superalloys. Fabrication methods for refractory-wire-superally
composites must be considered to be in the laboratory phase of development.
Production techniques for fabrication o f large numbers of specimens for exten-
sive property characterizations have not yet been developed.
Fabrlcation methods can be classified as either solid phase or liquid
phase depending upon the condition of the matrlx phase during its penetration
into a fibrous bundle. Liquid phase methods consists of casting the molten
matrix using Investment casting techniques so that the matrix infiltrates the
bundle of fibers in the form of parallel stacks or mats. The molten metal must
wet the fibers, form a chemical bond and yet be controlled so as not to
degrade the fibers by dissolution, reaction, or recrystallization.
Study and development of liquid phase fabrication techniques, (Ahmed and
Barranco, 1977; Glenny, 1970, and Morris and Burwood-Smith, 1971). has revealed
that large fibers and short liquld phase contact times are beneflcial. The
potential low cost of casting i s appealing but reaction induced fiber property
loss and limited fiber orientation control limit the applicability.
Solid phase processing requires diffusion, which Is time-temperature
dependent. Solid phase processing temperatures are much lower than liquid
phase processing temperatures; diffusion rates are much lower and reaction wlth
the fiber can be less severe. The prerequisite for solid state processing is
that the matrix be in either wire, sheet, foil, or powder form. Hot pressing
10
![Page 12: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/12.jpg)
or cold pressing followed by sintered i s used for consolidation of the matrix
and fiber into a composite component.
Use of matrix materials in the form of sheet or foil involves placing the
reinforcing fibers between layers of the matrix sheet or foil which are then
pressed together. They may be hot pressed or alternately cold pressed followed
by diffusion bonding. An example of this type of processing i s reported by
Karpinos et al. (1975). One of the most promising methods of manufacture of
composite sheet materials i s that o f vacuum hot rolling, which gives high pro-
ductivity and enables large sized sheets to be manufactured. A study was
reported of the processing parameters for the manufacture of composite sheet
material by vacuum hot rolling (Severdenko, 1974).
The powder metallurgy approach i s one of the most versatile methods for
producing refractory fiber-superalloy composites and has yielded some excellent
results. Almost all alloy metals can be produced in powder form. However, the
large surface area of the fine powders i s easily contaminated and introduces
impurities that must be removed. High capital cost equipment i s necessary t o
apply pressure and temperature in an inert atmosphere. Most powder-fabration
techniques limit fiber content to 40 to 50 vol X .
powder processing has been used to achieve control of matrix-fiber reactions
and has resulted in excellent composite properties.
Despite these disadvantages,
Slip casting o f metal alloy powders around bundles of fibers followed by
sintering and hot pressing was developed for the solid state fabrication of
refractory fiber-superalloy composites (Petrasek et al., 1968). Slipcast slur-
ries of a mixture of powders and an organic gel In water were used to form a
solid "green" composite which was subsequently sintered and then isostatically
hot pressed to full density. This method I s capable of achieving good matrix
consolidation and bonding between fiber and matrix without excursions into the
l l q u l d metal region which would greatly Increase fiber matrix reactions.
1 1
![Page 13: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/13.jpg)
Although thls technique has demonstrated excellent success for uniaxially rein-
forced specimens, it is not regarded as an ideal method for component fabrication
because most applications require some cross-ply fiber orientation, which is
not easily accomplished with slip casting.
A fabrication procedure was developed utilizing solid phase processing in
which fiber distribution, alignment, and fiber-matrix reaction could be accur-
ately controlled (Brentnall and Toth, 1974). Matrix alloy powders were blended
with a small quantity of organic binder (Teflon) and warm rolled into high
density sheets.
flbers whlch held the powder particles together. Fiber mats were made by wlnd-
Ing the fibers on a drum, and then spraying them with a binder. The fiber
array was cut from the drum and flattened to form a fiber mat. Precolllmated
fibers in mat form were sandwlched between layers of matrix powder sheet and
the material was densjfled and extruded between fibers by hot pressing. Fiber-
matrix and matrix-matrix metallurgical bonding was achieved while preservlng
uniform flber distribution and eliminatlng any voids. This procedure results
In the fabrication of a single layer of fibers contained In the matrix material
which was termed a monotape.
During rolling the Teflon formed an interlocklng'network of
Arc spraying represents the most versatile form o f compostte fabricatlon.
Arc spraying is a economical process for high temperature monotape fabrication
developed at NASA Lewls (Westfall, 1985), Flg. 6. Molten matrix alloy droplets
are sprayed I n a controlled atmosphere chamber onto a cylindrical drum wrapped
wlth fibers. The drum is rotated and translated within the chamber In front of
the spray to produced a controlled porosity monotape. Monotapes can then be
cut Anto any shape desired with any orientation of fiber deslred and sub-
sequently stacked up and hot pressed into any desired layup.
12
![Page 14: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/14.jpg)
IV. COMPOSITE PROPERTIES
The principal reason for most of the work on refractory fiber superalloy
composltes has been to produce a material capable of operation as h i g h l y
stressed components such as turbine blades In advanced aircraft and industrial
gas turbine engines at temperatures of 1100 to 1200 "C (2010 to 2190 O F ) or
higher. Such an increase i n temperature above the current limit of about
950 "C (1740 OF) for superalloy would permit higher turbine inlet temperatures
and markedly decreased cooling requirements, thus improving engine performance
and efficiency. An increase in blade temperature of 50 "C (90 O F ) over current
limits would be considered a significant improvement (Glenny, 1970).
of gas turbine blade material property requirements (Endres, 1974; Glenny and
Hopkins, 1976; and Stetson et al., 1966) indicates creep resistance, stress-
rupture strength, low-cycle fatigue, thermal fatigue resistance, impact
strength, and oxidation resistance as properties of primary concern for turbine
blade application. The following section reviews the results obtained for
refractory fiber/superalloy composites to meet these critical property
requirements.
A review
V. STRESS-RUPTURE STRENGTH
At temperatures of 1100 OC (2010 " F ) and above, a superalloy matrix con-
tributes very little to the rupture strength of the composite compared to the
contribution o f the refractory fibers. Fiber stress-rupture strength, volume
fraction of fiber, and the degree of fiber-matrix reaction all control the
stress-rupture strength of the composite. Figure 7 i s a plot comparing the
100 h r rupture strength at 1093 "C (2000 "F) for various fibers and composites
containing 70 vol X of these fibers (Petrasek and Signorelli, 1970 and 1974;
and Petrasek et al., 1968). The matrix composition (Ni-15Cr-25W-2Al-Ti) was
the same for all of the composites and as indicated in the plot, the stronger
the fiber the greater the stress-rupture strength of the composite. The effect
13
![Page 15: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/15.jpg)
of flber content on the stress-rupture strength of a composite is shown in
Fig. 8, (Dean 1967). Stress-rupture strength increases linearly as the fiber
content increases.
A cornparison of the 100 hr rupture strength at 1093 OC (2000 O F ) for some
of the composite systems that have been investigated, (Ahmad and Barranoio,
1977; Brentnall, 1976; Chubarov et al., 1972; Dean, 1967; Friedman and Fleck,
1979; Morris and Burwood-Smith, 1970; Petrasek and Signorelli, 1970 and 1974;
and Petrasek et al., 1968) is given in Table V and plotted in Fig. 9. Where
posslble, comparisons were made for composites containing 40 vol x fiber.
should be noted that higher values would be obtained for these composite systems
if the fiber content was increased. Also shown in the plot are the values for
the 100 hr rupture strength for unrelnforced alloys and for the strongest com-
mercially available superalloys. The 100 hr stress-rupture strength of all of
the alloys investigated was substantially increased by the addition of tungsten
fibers. All of the 40 vol % fiber composites had a 100 hr rupture strength
greater than that for the strongest commercially available superalloys. The
W-Hf-C flber composite system is the strongest composite systems obtained to
date. A 40 vol % w-Hf-C fiber content superalloy composite is over 3 and 1/2
tlmes as strong in rupture for 100 hr at 1100 "C (2010 OF) as the strongest
commerically available superalloys. The composite containing a larger amount
of fiber reinforcement (56 vol x W-1 percent Tho2 wire) in FeCrAlY also
had an impressive stress-rupture strength, over 2 and 1/2 times that for the
strongest commercially available superalloys.
The density of these composite materials is greater than that of super-
It
alloys and this factor must be taken into consideration. The stresses in tur-
bine blades, for e.g., are a result of centrifugal loading; therefore, the
density o f the materlal is Important. A comparison of the specific strength
properties of composites and superalloys i s therefore significant. Figure 10
14
![Page 16: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/16.jpg)
i s a pl t comp ring the values of the 1100 "C (2010 OF) 100 hr rupture strength
to density ratios for composites and superalloys.
density is taken into account, the stronger composites are still much superior
to the strongest commerically available superalloys. The composites containing
40 vol % W-Hf-C wire is almost 2 and 1/2 times as strong as the strongest
superalloys.
The plot shows that even when
The comparisons of stress-rupture strength between composites and super-
alloys i s even more favorable for the composite when long application times are
involved. Figure 1 1 is a plot of stress to rupture versus time t o rupture for
three different fiber compositions, each having the same matrix material, com-
pared to the strongest superalloys. All of the fiber composite systems are
stronger relative to superalloys for rupture in 1000 hr than for rupture in
100 hr at 1093 " C (2000 O F ) . The stress (to cause rupture) to density ratio
versus time t o rupture is plotted in Fig. 12. The specific stress-rupture
strength advantage for the composite also increases with time to rupture.
40 vol % tungsten fiber composite, e.g., has about the same specific (density
corrected) strength for rupture in 100 hr compared t o superalloys but is almost
twice as strong as superalloys for rupture in 1000 hr. For currently required
blade lives of 5 000 to 10 000 hr this advantage becomes even greater.
The
A comparison of the range o f values for the 100 hr rupture strength for
tungsten fiber reinforced superalloy composites tested at 1093 OC (2000 OF)
with the range for the stronger cast superalloys as a function of temperature
is shown in Fig. 13. The strongest TFRS composite has the same rupture strength
at 1093 "C (2000 O F ) as does the strongest superalloy at 915 "C (1680 OF).
This represents a material use temperature advantage for the composite o f 145 "C
(320 OF) compared to the strongest superalloy. Figure 14 shows the density cor-
rected values for rupture in 100 hr as a function o f temperature. When density
15
![Page 17: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/17.jpg)
i s t aken i n t o c o n s i d e r a t i o n t h e composl te has a m a t e r i a l use tempera tu re
advantage o f 110 " C (200 O F ) over t h e s t r o n g e s t s u p e r a l l o y s .
V I . CREEP RESISTANCE
The creep-rupture p r o p e r t i e s Nlmocast 713C r e i n f o r c e d w i t h t u n g s t e n o r
tungsten-5 p e r c e n t rhenium w i r e were eva lua ted and compared w i t h t h e d a t a
determined f o r vacuum-cast Nlmocast 713C, ( M o r r i s and Burwood-Smith, 1970) .
T y p i c a l composite creep curves a r e shown i n F i g . 15 t o g e t h e r w i t h a compar-
a t i v e curve f o r t h e u n r e i n f o r c e d m a t r i x . The creep curves f o r b o t h m a t e r i a l s
e x h i b i t t he t h r e e c h a r a c t e r i s t i c stages o f creep assoc ia ted w i t h c o n v e n t i o n a l
m a t e r i a l s . E s s e n t i a l l y , r e i n f o r c e m e n t reduces t h e second s tage minimum creep
r a t e markedly f o r a g l v e n a p p l i e d s t r e s s due t h e presence o f t h e more creep
r e s i s t a n t f i b e r s . The r e d u c t i o n i n minimum creep r a t e s observed on r e i n f o r c i n g
Nlmocast 713C suggests t h a t t h e s t ronger , more creep r e s i s t a n t component, t h e
f i b e r , c o n t r o l s t h e creep behav io r . The l a c k o f evidence o f creep d e f o r m a t i o n
i n t h e m a t r i x o f t h e composite, except a t t h e m a t r i x - f i b e r i n t e r f a c e a d j a c e n t
t o t h e f r a c t u r e su r face , a l s o suggested t h a t t h e behavqor i s c o n t r o l l e d by t h e
re in fo rcemen t .
r e i n f o r c e d H a s t e l l o y X composi tes (Baskey, 1967), tungsten-1 p e r c e n t Tho2
r e i n f o r c e d FeCrAlY composi tes ( B r e n t n a l l , 1976), and w i t h t u n g s t e n - n i c k e l
composites (Kannappan and F i schme is te r , 1975).
V I I . FATIGUE
S i m j l a r r e s u l t s were ob ta ined w i t h tungsten-1 p e r c e n t Tho2
High-temperature m a t e r i a l s i n gas t u r b i n e s a r e s u b j e c t t o c y c l i c s t r e s s e s
and s t r a i n s . These can l e a d t o t h e development o f cracks and f a i l u r e s which
c o n v e n t i o n a l l y a r e d i scussed i n t h r e e separate groupings, depending on t h e
magnitude and cause o f t h e s t r e s s e s :
H lgh -cyc le f a t i g u e
Low-cycle f a t i g u e
16
![Page 18: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/18.jpg)
Thermal f a t i g u e
( a ) H igh Cycle F a t i g u e
H igh -cyc le f a t i g u e t e s t s have been conducted on W-1 p e r c e n t Th02 /Has te l l oy
X composi te specimens (Baskey, 1967). f a t i g u e t e s t s were performed u s i n g
d i r e c t s t r e s s , t e n s i o n - t e n s i o n , a x i a l l y loaded specimens. The s t r e s s t o cause
f a i l u r e i n 1x10 c y c l e s versus temperature i s p l o t t e d i n F i g . 16. U n r e i n f o r c e d
H a s t e l l o y X d a t a a r e p l o t t e d f o r comparison. The composi tes were s t r o n g e r a t
a l l temperatures, r a n g i n g f r o m 1.2 t i m e s as s t r o n g a t room temperature t o 4
t imes as s t r o n g a t 980 " C (1800 O F ) . The r a t i o o f f a t i g u e s t r e n g t h t o u l t i m a t e
t e n s i l e s t r e n g t h f o r t h e same m a t e r i a l s I s p l o t t e d i n F i g . 17. For a l l t e s t
temperatures, t h e r a t i o f o r t h e composite was h i g h e r than t h a t f o r t h e
H a s t e l l o y X, i n d i c a t i n g t h a t h igh -cyc le f a t i g u e r e s i s t a n c e o f t h e composi te i s
c o n t r o l l e d by t h e f i b e r .
6
The h i g h - c y c l e f a t i g u e s t r e n g t h f o r W-1 p e r c e n t Th02/FeCrA1Y composi tes
was determined a t 760 and 1039 O C (1400 and 1900 O F ) I n ( F l e c k , 1979). F a t i g u e
t e s t s were per formed u s i n g d i r e c t t ens ion - tens ion , a x i a l l y loaded specimens.
F i g u r e 18 i s a p l o t o f maximum s t r e s s versus t h e number o f c y c l e s t o f a i l u r e
f o r specimens t e s t e d a t 760 " C (1400 "F). The maximum s t r e s s versus number o f
c y c l e s t o f a i l u r e f o r specimens t e s t e d a t 1038 O C (1900 O F ) i s p l o t t e d i n
F i g . 19. The r e s u l t s a g a i n i n d i c a t e t h a t f a t i g u e i s c o n t r o l l e d by t h e f i b e r .
6 F i g u r e 20 i s a p l o t o f t h e 1x10
tens l e s t r e n g t h r a t i o f o r some supera l l oys and t h e range o f va lues o b t a i n e d
f o r FRS composi tes showing t h a t t h e composites' response t o h i g h - c y c l e f a t i g u e
I s s u p e r i o r t o t h a t f o r s u p e r a l l o y s . Push/pul l and r e v e r s e bend f a t i g u e
s t r e n g t h d a t a were determined f o r a W/superal loy composi te (Dean, 1967) . The
f a t i g u e s t r e n g t h measured i n p u s h / p u l l t e s t s a t 20, 300, and 500 O C (70, 570,
and 930 O F ) was s u b s t a n t i a l l y increased by t h e i n t r o d u c t i o n o f 40 v o l X
c y c l e f a t i g u e s t r e n g t h t o u l t i m a t e
17
![Page 19: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/19.jpg)
tungsten wlres. With cantilever specimens tested in reverse bending, a
slgniflcant increase In fatigue strength also resulted from the incorporatlon
of tungsten wires.
(b) Low-Cycle Fatigue
Limited work has been reported on the low cycle fatlgue behavior of
refractory fiber/superalloy composites. The low cycle fatlgue behavlor for
tungsten flber reinforced nickel was determined at room temperature (Nllsen
and Sovik, 1974). Specimens containing 1 1 t o 25 vol %, 500 pm (0.020 In.)
diameter, tungsten flbers or 20 t o 28 vol X , 100 pm (0.004 In.) dlameter,
tungsten fibers were fabricated by a llquld metal Inflltratlon process and
tested in fatlgue. Speclmens containing 8 or 10 vol % of 300 pm (0.012 in.)
diameter tungsten fibers were fabricated by a powder and subsequent forging
process and also tested In fatigue. Fatigue tests were performed at about
150 Hz using direct stress, tenslon-tension, axially loaded specimens.
Figure 21 i s a plot of the ratlo of the maxlmum stress for fatigue failure to
ultimate tensile strength for the range of cycles investlgated. The observed
fatigue ratios shown for the com- posite specimens were much higher in cornpar-
ison to some superalloys referenced by the author. The fatigue ratlo reported
for Nimocast 713C for 10 cycles was 0.24 and for Incoloy 901 and Udimet 700
for 10 cycles the ratio was 0.14 and 0.17, respectively. As shown in Fig. 21
the fatigue ratio obtained for the composites was greater than 0.65 at 10
cycles.
8
7
6
Low-cycle fatigue tests were conducted at 760 and 980 O C (1400 and 1800 OF)
on 20 and 35 vol % W-1 percent Tho fiber reinforced FeCrAlY composltes,
(Fleck, 1979). Fatigue tests were performed at 0.65 H z and a stress cycle of
from 5.5 MN/m (0.8 ksl) to a maxlmum stress. The load ratio, R , was -0.01
and the stress ratlo, A , was 1 . The low-cycle fatigue results are plotted ln
Fig. 22. The results indicate that the flber controls low cycle fatlgue
2
2
18
,
![Page 20: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/20.jpg)
strength as was the case for high-cycle fatigue behavior. The 35 vol % fiber
content specimens had much higher values of fatigue strength versus cycles to
failure than did the 20 vol X percent fiber specimens. The ratio of fatigue
strength to ultimate tensile strength versus cycles to failure is plotted i n
Fig. 23. Very high values were obtained at both 760 and 980 "C (1400 and
1800 O F ) indicating that the composite has a higher resistance to low cycle
fatigue in this temperature range.
(c) Thermal Fatigue
Thermal fatigue failures are caused by the repeated application of stress
that is thermal in origin. Rapid changes in the temperature of the environment
can cause transient temperature gradients i n components. Such temperature
gradients give rise to thermal stresses and strains. Thermal fat
i s the cracking o f materials caused by repeated rapid temperature
Superimposed on stresses generated by temperature gradients,
of the composite, are internal stresses caused by the difference
coefficients between the fibers and matrlx. The mean coefficient
gue failure
changes.
in the case
n expansion
of thermal
expansion from room temperature to 1100 O C (2010 O F ) for superalloys ranges
from 15.8 t o 1 9 . 3 ~ 1 0 /"C (8.8 to 10.7~10-~/"F) and is - 5 ~ 1 0 - ~ / " C (2.7~10-
for tungsten. Because of the large difference in expansion coefficients
between the fiber and matrix and the resulting strains, thermal fatigue is
believed to be the most serious limitation on composite usefulness.
6 6 OF)
A number of investigators have developed analytical methods to calculate
the dependence of composite deformation on cyclic, geometric, and constituent
deformation parameters (Baranov and Yakovleva, 1975; Gaiduk et al, 1972; and
Garmong, 1974). The results of these calculations illustrate the possible
effects of several variables on deformation damage parameters. Because of the
dlfference i n expansion coefficients, the matrix is strained in tension upon
19
![Page 21: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/21.jpg)
cooling and in compression upon heating while the fiber is strained in compres-
sion upon cooling and tension upon heating.
Work reported by Garmong (1979), indicates that the hystersis loop of matrix
stress versus temperature caused by plastic deformation of the matrix due to
the heating and cooling cycle stabilizes after a few cycles so that a steady-
state plastic compression-tension fatigue results when no external stress is
present. Total cyclic plastic strain increases by a law of the form, total
strain = strain per cycle x number of cycles. The ability o f the matrix to
accommodate plastic strain thus controls the number of cycles to failure for
the composite if plastic deformation of the matrix governs the failure mode of
the composite in fatigue.
Three types of cycling damage have been noted to date: plastic flow of the
fiber in compression, matrix fracturing and fiber-matrix interface debonding.
A number of studies have been conducted on the response of tungsten fiber/
superalloy composites to thermal cycling. Table V I compares the data obtained
for several composite systems. Cylindrical specimens of 40 percent W/Nlmocast
258 were cycled between room temperature and 1100 O C (2010 O F ) in a fluidized
bed to obtain rapid heating and cooling, (Dean, 1967). Metallographic examin-
ation after 400 cycles revealed no apparent damage at the fiber-matrix inter-
face. Cylindrical specimens of W/Nimocast 713C were cycled in a fluidized bed
in the temperature ranges shown in Table V , (Morris and Burwood-Smith, 1971).
Cracking occurred after relatively few cycles with the exception of the speci-
mens cycled from 20 to 600 "C (70 to 1110 OF). The bond between the fiber and
matrix was reported t o be severely degraded by thermal cycling to 1050 "C
(1920 O F ) .
20
![Page 22: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/22.jpg)
Thermal c y c l e t e s t s were conducted on specimens o f r e i n f o r c e d sheet
m a t e r i a l hav ing a m a t r i x o f € 1 4 3 5 (Nichrome) (Dudnik e t a l . , 1973) . The s p e c i -
mens were heated i n an e l e c t r i c r e s i s t a n c e f u r n a c e f o r 2.5 m in up t o a temper-
a t u r e o f 1100 O C (2010 O F ) f o l l o w e d by a water quench t o room temperature. The
number o f c y c l e s f o r debonding between t h e f i b e r and m a t r i x t o occur was d e t e r -
mined as a f u n c t i o n o f f i b e r c o n t e n t . As shown I n Table V t h e number o f c y c l e s
f o r debonding t o occur decreased w i t h I n c r e a s i n g f i b e r c o n t e n t .
Tests were a l s o conducted on r e i n f o r c e d E 1 4 3 5 sheet m a t e r i a l by Banas
e t a l . (1976) . The specimens were heated by passage o f an e l e c t r i c c u r r e n t .
I r r e v e r s i b l e d e f o r m a t i o n occu r red a f t e r c y c l i n g f o r a l l o f The 15 volume f i b e r
c o n t e n t specimens b u t n o t f o r t h e 32 volume f i b e r c o n t e n t specimens.
t h e i n i t i a l stages o f c y c l i n g , warpage and bending were observed. A l e n g t h
decrease was observed d u r i n g t h e e n t i r e t e s t . W i th an i n c r e a s e o f t h e number
o f c y c l e s t h e l e n g t h and r a t e o f t h e dimensional change d im in i shed . Heat t r e a t -
ment had a c o n s i d e r a b l e e f f e c t on dimensional i n s t a b i l i t y o f t h e composi te. As
a r e s u l t o f a n n e a l i n g t h e specimen t h e i r p r o p e n s i t y f o r de fo rma t ion d u r i n g
t h e r m o c y c l i n g decreased. Anneal ing reduced t h e y i e l d s t r e n g t h o f t h e m a t r i x .
The l e v e l o f s t r e s s e s a r i s i n g i n t h e f i b e r s as a consequence o f t h e d i f f e r e n c e
i n expansion c o e f f i c i e n t s was determined by t h e r e s i s t a n c e t o p l a s t i c deform-
a t i o n o f t h e m a t r i x . W i t h a decrease I n t h e y i e l d s t r e n g t h o f t h e m a t r i x t h e
l e v e l o f s t r e s s on t h e f i b e r decreased and t h e f i b e r s d i d n o t p l a s t i c a l l y
deform.
D u r i n g
Severa l d i f f e r e n t n i c k e l base composite systems were t h e r m a l l y c y c l e d i n
work r e p o r t e d by U r e n t n a l l and Moracz (1976). Specimens were heated by passage
o f an e l e c t r i c c u r r e n t . The specimens were heated t o 1093 "C (2000 O F ) i n 1 min
and c o o l e d t o room temperature i n 4 m i n . A l l of t h e 35 volume f i b e r c o n t e n t
specimens were warped a f t e r 100 cyc les , w h i l e t h e 50 vo
mens were n o t . The most d u c t i l e m a t r i x m a t e r i a l s N l C r A Y showed t h e l e a s t
% f i b e r c o n t e n t spec i -
21
![Page 23: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/23.jpg)
amount o f damage a f t e r 100 c y c l e s . Specimens c o n t a i n i n g 30 v o l x W-1 p e r c e n t
Tho f i b e r s i n a m a t r i x o f FeCrAlY were exposed t o 1000 c y c l e s f r o m room tem-
p e r a t u r e t o 1204 O C (2200 O F ) , ( B r e n t n a l l e t a l . , 1975) .
heated up t o 1204 O C (2200 O F ) i n 1 min and cooled t o room temperature i n 4 min.
A s shown In F i g . 24, s u r f a c e roughening occurred, b u t t h e r e was no m a t r i x o r
f i b e r c r a c k i n g a f t e r t h e 100 c y c l e exposure.
2
The specimens were
A s i n d i c a t e d i n Table V I , a composi te system has been i d e n t i f i e d , W-1
Th02/FeCrA1Y, t h a t can be t h e r m a l l y c y c l e d though a l a r g e number o f c y c l e s
w i t h o u t any apparen t damage.
258 composite system which w i t h s t o o d 400 c y c l e s w i t h o u t any apparent damage,
a l l o f t he o t h e r systems i n v e s t i g a t e d i n d i c a t e d t h a t some t y p e of damage
occurred.
would be exposed t o ve ry few the rma l c y c l e s . Only a l i m i t e d number of systems
have been i n v e s t i g a t e d t o d a t e and a need e x i s t s t o i d e n t i f y o t h e r the rma l
f a t i g u e r e s i s t a n t systems.
which can r e l l e v e t h e r m a l l y induced s t r a i n s by p l a s t j c de fo rma t ion i s r e q u i r e d
f o r composite thermal f a t i g u e r e s i s t a n c e .
W i t h t h e e x c e p t i o n o f t h e 40 p e r c e n t W/Nimocast
These systems would be l i m i t e d t o a p p l i c a t i o n s where t h e component
The r e s u l t s ob ta ined i n d i c a t e t h a t a d u c t i l e m a t r i x
VIII. I M P A C T STRENGTH
Composite mater ’ ia ls must be capable o f r e s i s t i n g impact f a i l u r e f r o m
f o r e i g n ob jec ts o r f r o m f a i l e d components t h a t may pass th rough t h e eng ine i f
t h e y a r e t o be cons ide red f o r use as a i r c r a f t engine b l a d e o r vane components.
Factors a f f e c t i n g t h e impact s t r e n g t h o f t ungs ten f i b e r me ta l m a t r i x com-
p o s i t e s were i n v e s t i g a t e d by Winsa and Petrasek (1973).
s tandard Charpy impact s t r e n g t h d a t a were ob ta ined f o r a t u n g s t e n f i b e r r e i n -
f o r c e d n i c k e l base a l l o y (N1-25W-15Cr-2Al-Ti). I t has been found t h a t compos-
i t e p r o p e r t i e s as measured by t h e m i n i a t u r e I z o d impact t e s t c o r r e l a t e c l o s e l y
w i t h composite p r o p e r t i e s as measured by v a r i o u s b a l l i s t i c impact t e s t s and I t
was concluded t h a t t h e m i n i a t u r e Izod t e s t i s a reasonable sc reen ing t e s t f o r
M i n i a t u r e I z o d and
22
![Page 24: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/24.jpg)
candidate turbine blade and vane materlal (Ohnysty and Stetson, 1967). The
Izod impact strength of unnotched and notched specimens as a function of fiber
content is plotted in Fig. 25 for two test temperatures, (75 and 1000 OF).
Impact strength decreased with increasing fiber content at the lower temperature,
but increased with increasing fiber content at the higher temperature.
Figure 25 1s a plot of Impact strength as a function of temperatures.
4 s a sharp increase in Impact strength for the 60 vol x unnotched specimens
at 260 "C (500 O F ) , which correspond to the ductile-brittle transition tem-
perature (DBTT) for the fiber. In general, unnotched composites had higher
impact strength, compared to the matrix, at temperature above the DBTT of the
fiber and lower tmpact strength than the matrix below the DBTT of the fiber.
The matrix's contribution to impact strength for the composite is most signi-
ficant at low temperatures, while the fiber controls higher temperature impact
strength, above 260 O C (500 OF).
tivity was also determined. The ratio of the composite's notched impact
strength per unit area to its unnotched impact strength per unit area is
plotted as a function of fiber content in Fig. 27.
the composite decreased with increasing fiber content both above and below the
DBTT of the fiber. Heat treatment or hot rolling improved the room tempera-
ture impact strength of the composite. Heat treatment increased the impact
strength of the notched unreinforced matrix by almost four times and nearly
doubled the impact strength of a 45 vol X fiber content composite.
increased the impact strength of a 56 vol X fiber content composite by nearly
four times. The improved impact strength for the composite was related to
improved matrix impact strength.
There
The effect of fiber content on notch sensi-
The notch sensitivity of
Rod rolling
An additional objective of work conducted by Winsa and Petrasek (1973) was
to determine if the potential impact resistance of tungsten fiber/superal loy
composites was sufficient to warrant their consideration as turbine blade o f
23
![Page 25: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/25.jpg)
vane m a t e r i a l s . A l l o y s w i t h m i n i a t u r e I z o d impact values l e s s than 1 . 7 J
( 1 5 i n . - / b ) have been s u c c e s s f u l l y r u n as t u r b i n e b lades ( S i g n o r e l l i e t a l . ,
1956; and Waters e t a l . , 1959). Based on t h i s , t h e va lue o f 1.7 J (15 1n . - l b )
was taken as t h e minimum va lue f o r I z o d impact s t r e n g t h t o I n d i c a t e i f a mate-
r l a l has promise f o r f u r t h e r e v a l u a t i o n l e a d i n g t o t u r b i n e b lade use.
F i g u r e 28 compares t h e tungs ten f l b e r / s u p e r a l l o y impact s t r e n g t h va lues w t t h
t h e minimurn s tandard .
f l b e r conten ts g r e a t e r t han 35 pe rcen t d i d n o t meet t h e minimum requ i rement .
Heat t rea tmen t and h o t work ing , however, Improved t h e impact s t r e n g t h so t h a t
h l g h f i b e r c o n t e n t composites met t h e minlmum requ i rements .
(1400 O F ) , t h e h l g h e r f i b e r c o n t e n t a s - f a b r i c a t e d composites have impact
s t r e n g t h s d i s t i n c t l y above t h e minimum requ i rement .
s t r e n g t h values were ob ta ined a t 1093 C (2000 O F ) , 37.3 J (330 i n . - l b ) f o r a
60 vol % f t b e r c o n t e n t specimen, i m p l y ng t h a t most o f t h i s s t r e n g t h i s main-
t a i n e d t o a t l e a s t 1093 O C (2000 O F ) .
s t e n f i b e r / s u p e r a l l o y composites thus appears adequate f o r some a l r c r a f t engine
component a p p l i c a t i o n s , such as t u r b i n e a i r f o i l s and vanes.
A t room tempera ture a f a b r i c a t e d composites c o n t a l n i n g
A t 760 "C
High Charpy impact
The Impact s t r e n g t h p o t e n t i a l f o r tung-
I X . O X I D A T I O N AND CORROSION
The gaseous env l ronment i n t h e gas t u r b i n e engine i s h i g h l y o x i d i z i n g w i t h
oxygen p a r - t i a l p ressu re o f t h e o r d e r o f 2 t o 4 atm, (El-Dahshan e t a l . , 1975).
However, t h i s env i ronment a l s o c o n t a i n s s i g n i f i c a n t amounts o f combustion
p roduc t I m p u r i t i e s i n c l u d i n g s u l f u r f rom t h e f u e l and a l k a l t s a l t s I nges ted
w i t h t h e i n t a k e a i r . Under these c o n d i t i o n s an a c c e l e r a t e d o x i d a t i o n may be
encountered, sometimes, b u t n o t always, accompanied by t h e f o r m a t i o n o f
s u l f i d e s w i t h l n t h e a l l o y : t h i s I s commonly r e f e r r e d t o as hot c o r r o s i o n .
The b a s i c des lgn o f t h e composite m a t e r i a l assumes t h a t t h e s u p e r a l l o y
m a t r i x w i l l p r o v l d e o x i d a t i o n r e s i s t a n c e , i n c l u d i n g p r o t e c t i o n o f t h e t u n g s t e n
I
I
I
I I
I
I I I
I
I
i J I
i i
24
![Page 26: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/26.jpg)
f i b e r s .
t i o n r e s i s t a n t f o r m a t e r i a l o p e r a t i n g temperatures up t o about 980 O C (1800 O F ) .
Above a m a t e r i a l tempera ture of 980 " C (1800 O F ) i t i s necessary t o c o a t or
c l a d t h e m a t e r i a l t o p r o v i d e t h e requ i red o x i d a t i o n r e s i s t a n c e .
a r e used f o r s u p e r a l l o y o x i d a t i o n p r o t e c t i o n , such as N i C r A l Y and FeCrAlY, a r e
o x i d a t i o n r e s i s t a n t t o temperatures above 1090 " C (2000 OF). These m a t e r i a l s
may a l s o be cons idered as t h e m a t r i x for composites so t h a t t h e composi te would
n o t have t o be coated or c l a d f o r h i g h temperature ox d a t i o n r e s i s t a n c e . Pre-
l i m i n a r y o x i d a t i o n s t u d i e s were conducted on a n i c k e l base s u p e r a l l o y r e i n -
f o r c e d w i t h tungsten-1 p e r c e n t Tho2 f i b e r s and c l a d w t h Incone l by Petrasek
and S l g n o r e l l i (1970).
f o r t imes up t o 300 h r .
specimen exposed f o r 50 hr a t 1093 O C (2000 O F ) .
o x i d i z e d , and a coherent o x i d e s c a l e formed on t h e I n c o n e l . O x i d a t i o n had n o t
progressed t o t h e composi te , and t h e surface f i b e r s were n o t a f f e c t e d by t h e
o x i d a t i o n o f t h e c l a d d i n g . Composite specimens of W-1 pe rcen t Tho /FeCrAlY
hav ing comp le te l y m a t r i x p r o t e c t e d f i b e r s were exposed t o s t a t i c a i r a t 1038,
1093, and 1149 O C (1900, 2000, and 2100 O F ) f o r up t o 1000 h r . The we igh t
change i n 1000 h r was 0.3 mg/cm f o r 1038 O C (1900 O F ) and 1.25 mg/cm f o r
1149 O C (2100 O F ) . These va lues a r e i n agreement w i t h va lues ob ta ined f o r t h e
m a t r i x m a t e r i a l w i t h o u t any re in fo rcement (Wukusick, 1966). O x i d a t i o n d i d n o t
p rogress t o t h e s u r f a c e f i b e r s .
Supera l l oys t h a t a r e used f o r h o t s e c t i o n engine components a r e ox ida -
Claddings t h a t
The specimens were exposed i n a i r a t 1093 O C (2000 O F )
F i g u r e 29 i s a t ransve rse s e c t i o n o f a c l a d composi te
The I n c o n e l c l a d d i n g was
2
2 2
The o x i d a t i o n and c o r r o s i o n res i s tance o f composite m a t e r i a l s hav ing
exposed f i b e r s i s a l s o an i m p o r t a n t cons ide ra t i on . A l though t h e f i b e r s i n t h e
composite would n o t be des lgned t o be exposed t o t h e engine env i ronment an
unders tand ing o f t h e h i g h tempera ture o x i d a t i o n and c o r r o s i o n behav io r i s
d e s i r a b l e i n t h e even t o f a c o a t i n g , c ladding, o r m a t r i x f a i l u r e d u r i n g s e r v i c e
whlch c o u l d occur, e.g., f rom impact due t o f o r e i g n o b j e c t s pass ing th rough t h e
25
![Page 27: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/27.jpg)
engine.
of exposed f i b e r s .
t h e b lade o r vane t h i c k n e s s ) would d e s t r o y t h e exposed f i b e r s , b u t i n t e r v e n i n g
m a t r i x would p r e v e n t o x i d a t i o n o f subsequent l a y e r s .
l o s s o f s t r e n g t h would r e s u l t .
b lade o r vane span) p o t e n t i a l l y i s more severe, s i n c e a l l t h e exposed f i b e r s
i n t h e t ransverse s e c t i o n p o t e n t i a l l y cou ld be o x i d i z e d a long t h e i r e n t i r e
l e n g t h .
o n l y l i m i t e d o x i d a t i o n p e n e t r a t i o n a long t h e f i b e r s ( B r e n t n a l l e t a l . , 1975;
Dean, 1965; and El-Dahshan e t a l . , 1975).
F igure 30 i l l u s t r a t e s t h e p r i n c i p a l paths f o r o x i d a t i o n and c o r r o s i o n
O x i d a t i o n proceed ing pe rpend icu la r t o t h e f i b e r s ( t h r o u g h
Thus, o n l y a p a r t i c a l
O x i d a t i o n p a r a l l e l t o t h e f i b e r s ( a l o n g t h e
However, s t u d i e s conducted t o eva lua te o x i d a t i o n a long f i b e r s showed
The hot c o r r o s i o n behav io r o f tungs ten f i b e r r e i n f o r c e d Ni-20 pe rcen t C r
composite specimens was a l s o examined by El-Dahshan e t a l . (1975). under t h e
f o l l o w i n g exposure c o n d i t i o n s :
p r e s u l f i d a t i o n i n H2-10 pe rcen t H2S f o l l o w e d by o x i d a t i o n i n oxygen; and ( c )
o x i d a t i o n i n 1 atmosphere o f oxygen a f t e r p r e c o a t i n g w i t h Na2S04.
f i d a t i o n , on ly t h e m a t r i x formed s u l i f i e d and t h e f i b e r s remained u n a f f e c t e d .
Consequently, p r e s u l f i d a t i o n , a l t hough hav ing a d ramat ic e f f e c t on t h e ox ida -
t i o n o f the m a t r i x d i d n o t have a damaging e f f e c t on t h e f i b e r s .
o f sodium s u l f a t e was a l s o n o t c r i t i c a l . Thus, h o t c o r r o s i o n c o n d i t i o n s were
n o t harmful t o t h e t u n g s t e n r e i n f o r c e d composites s t u d i e d , and c a t a s t r o p h i c
l o s s o f the exposed tungs ten f i b e r s d i d n o t occur upon exposure t o a h igh -
temperature o x i d i z i n g e n v i ronment.
( a ) s u l i f i d a t i o n i n H2-10 pe rcen t H2S; (b)
Dur ing s u l i
The p resen ts
X . THERMAL C O N D U C T I V I T Y
High thermal c o n d u c t i v i t y i s d e s i r a b l e i n a t u r b i n e b lade m a t e r i a l t o
reduce temperature g r a d i e n t s ; t h i s , i n t u r n , r e s u l t s i n reduced t h e r m a l l y
induced s t r a i n s t h a t can cause c racks o r d i s t o r t i o n . I n a d d i t i o n , h i g h e r
thermal c o n d u c t i v i t y can reduce c o o l a n t f l o w requ i rements i n some impingement
![Page 28: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/28.jpg)
cooled blades leading to greater engine efficiency or durability (Winsa
et al., 1978).
The conductivity of tungsten fiber/superalloy composites is markedly
superior to that of superalloys.
higher that for superalloys and the more tungsten added to a composite the
greater the conductivity. Thermal conductivity of the composite is greatest in
the direction of the fiber axes since there is a continuous path for conduction
along the tungsten fibers. Conduction perpendicular to the fiber axes is lower
because the heat cannot find a continuous path through tungsten. The thermal
conductivity of some tungsten fiber/superalloy composites was determined as a
function of temperature by Wlnsa et al. (1978). Figure 31 shows the thermal
conductivity values obtained for a composite containing 65 vol % fibers i n a
nickel base alloy and tested in the direction of the fiber axis and for a com-
posite containing 50 vol % and tested i n the direction perpendicular the fiber
axis. The longitudinal thermal conductivity is seen to be much higher than the
transverse conductlvity.
materials. The composites have much higher values for thermal conductivity
over the entire temperature range.
The thermal conductivity of tungsten is much
Also shown i n the figure are values for the matrix
Composite Component Fabrication
Having demonstrated adequate properties for application as a turbine blade
material, the next area of considerat1,on is whether complex shapes such as
hollow turbine blades can be designed and fabricated from such material and at
reasonable cost. The selected composite fabrication technqiues must result i n
a composite whose properties meet those required for application of the com-
posite.
required dimensions, second Incorporating both uniaxial and off-axis fiber
The processes must be capable of first producing component shapes to
27
![Page 29: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/29.jpg)
p o s i t i o n i n g ; t h i r d p r o v i d i n g u n i f o r m m a t r i x c l a d d i n g t o p r e v e n t f i b e r o x i d a -
t l o n , and f o u r t h , p r o v i d i n g i f necessary, f o r c o o l l n g o r w e i g h t r e d u c t l o n pass-
ages.
r e p r o d u c 1 b 1 e.
The combined f a b r i c a t i o n technlques must a l s o be c o s t e f f e c t i v e and
D l f f u s i o n bonding o f monolayer composi te p l i e s l s c u r r e n t l y t h e most prom-
i s l n g , c o s t e f f e c t i v e method o f f a b r i c a t l o n f o r complex shapes.
p l i e s c o n s i s t o f a l i g n e d tungs ten f l b e r s sandwiched between l a y e r s o f m a t r l x
m a t e r i a l . Th i s approach has t h e c a p a b l l i t y f o r a c c u r a t e f i b e r d l s t r i b u t i o n
and a l ignment ; moreover, i t l l m i t s f i b e r - m a t r l x i n t e r d i f f u s i o n d u r i n g f a b r l c a -
t l o n . This approach a l s o i s capable of p r o d u c i n g b lade shapes t h a t a r e c l o s e
t o f l n a l dlmenslons; hence, o n l y l l m l t e d machin ing and touch up g r i n d i n g i s
needed (Mazzei e t a l . , 1976; Melnyk and F leck , 1979; and Petrasek e t a l . ,
1979) .
The composi te
The f e a s i b i l i t y o f composl te component f a b r i c a t i o n , was s u c c e s s f u l l y dem-
o n s t r a t e d (Melnyk and F leck , 1979) . A JT90-7F f i r s t stage, c o n v e c t i o n coo led
t u r b i n e blade was s e l e c t e d as t h e model f r o m which a W-1 p e r c e n t Th02/FeCrA1Y
composi te blade was designed.
n o t o n l y t o demonstrate t h e f e a s i b i l i t y o f f a b r i c a t i n g a complex shape b u t t o
a l s o demonstrate t h a t des ign requi rements c o u l d be met i n t h e f a b r i c a t e d
b lade . The des ign f e a t u r e s i n c o r p o r a t e d i n t o t h e f a b r l c a t e d b l a d e a r e
i n d l c a t e d I n F i g s . 32 and 33.
The major purpose o f t h e f a b r i c a t l o n e f f o r t was
F igu re 34 shows t h e f a b r l c a t l o n sequence used t o produce t h e h o l l o w com-
p o s i t e t u r b i n e b l a d e . A t u n g s t e n f i b e r mat was sandwiched between powder
sheets of FeCrAlY which was subsequent ly h o t pressed t o f o r m a monotape. The
monotape was t hen c u t i n t o t h e p l i e s necessary t o a r r i v e a t t h e f i n a l b l a d e
dimension. The p l i e s wee t h e n s tacked around a s t e e l co re . Root i n s e r t s and
o u t s e r t s could a l s o be s tacked around t h e assembly o r c o u l d be a t t a c h e d i n a
28
![Page 30: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/30.jpg)
secondary f a b r i c a t t o n s tep . The e n t i r e assembly was t h e n p laced i n a r e f r a c -
t o r y m e t a l d i e , heated and pressed t o a r r i v e a t t h e p roper a i r f o i l c o n t o u r .
A f t e r p r e s s i n g t h e s t e e l c o r e was removed by l e a c h i n g o u t w i t h an a c i d . A t i p
cap was t h e n was welded on t o t h e end of t h e a i r f o i l and an impingement c o o l i n g
i n s e r t was p l a c e d i n he leached o u t c a v l t y and brazed i n t h e r o o t o f t h e b lade .
F l g u r e 35 shows t h e as f a b r i c a t e d W-1 pe rcen t Th02/FeCrA1Y composi te
h o l l o w JT9D-7F a i r f o i l c o n t a i n i n g a bonded on end cap and t r a i l i n g - e d g e c o o l a n t
s l o t s . F i g u r e 36 shows t h e composi te a i r f o i l which was brazed t o a h i g h s t r e n g t h
s u p e r a l l o y a r c r o o t . A c ross s e c t i o n of t h e composi te a i r f o i l i s shown i n
F i g . 37. E x c e l l e n t f i b e r a l i gnmen t and f i b e r d i s t r i b u t i o n was o b t a i n e d and
t h e f i b e r s were f u l l y p r o t e c t e d by a l a y e r o f FeCrAlY on t h e i n t e r i o r and
e x t e r i o r s u r f a c e s o f t h e a i r f o i l .
Success fu l f a b r i c a t i o n o f a h o l l o w composi te a i r f o i l has demonstrated t h a t
t h i s m a t e r i a l can be f a b r i c a t e d i n t o the complex d e s i g n shapes f o r h o t t u r b i n e
s e c t i o n components. Whi le components such as vanes o r combustion l i n e r s have
n o t been f a b r i c a t e d these components are l e s s complex than t h e b l a d e and can
be cons ide red f o r f u t u r e programs.
The f a b r i c a t i o n process sequence used t o produced a h o l l o w composi te b l a d e
was used i n a f a b r i c a t i o n c o s t s tudy (Bar th e t a l . , 1977) . F a b r i c a t i o n c o s t s
were e s t i m a t e d f o r h i g h technology t u r b l n e b l a d e f a b r i c a t e d u s i n g t h e e d i f f e r -
e n t m a t e r i a l s . The same t u r b i n e b lade c o n f i g u r a t i o n , a f i r s t s tage JT9D-7F b l a d e
was used f o r each m a t e r i a l . D i r e c t i o n a l l y s o l i d i f i e d e u t e c t i c (DSE), an o x i d e
d i s p e r s i o n s t reng thened s u p e r a l l o y (ODSS), and W-1 p e r c e n t Tho /FeCrAlY b l a d e
manu fac tu r ing c o s t s were compared w i t h the c o s t o f p roduc ing t h e same b l a d e f r o m
a d i r e c t i o n a l l y s o l i d i f i e d (DS) supera l l oy , t h e c u r r e n t b l a d e m a t e r i a l . The
r e l a t i v e c o s t s a r e shown i n Fig. 38. The s tudy i n d i c a t e s t h a t W/FeCrAlY
2
29
![Page 31: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/31.jpg)
manufacturlng cost should be competitive with current manufacturing costs of
manufacturlng this blade by directional solidlflcation of a superalloy-
provided the projected manufacturing yields can be realized in actual
commerical production of blades.
XI. CONCLUDING REMARKS
Exploratory development and material property screening have indicated
that tungsten fiber reinforced superalloy composites have considerable poten-
tial for application as advanced high temperature material. Studies o f a wide
range o f physlcal and mechanial properties in laboratory tests have demon-
strated the advantage of tungsten flber reinforced superalloy composites over
conventional superalloys. Also computer simulations and evaluations of super-
alloy composite performance as engine components have indicated the potentlal
for significant temperature and strength increases. Moreover, blade fabrica-
tion studjes have demonstrated the feasibility of producing complex hollow
shapes at a cost competitive wlth directionally solidified superalloy blade
costs. Still, a great deal of work remains to be done on this family of mater-
ials to ald in its transition from laboratory feasibility to rig testing of
prototype hardware and then on manufacturing technology and detailed design.
30
![Page 32: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/32.jpg)
REFERENCES
1. Ahmad, I., and Barranco, J.M. (1977). SAMPE Q. E l , 38-49.
2. Amra, L.H., e t a l . (1970) . "Development o f F a b r i c a t i o n Process f o r
3. Banas, F.P., Baranov, A.A., and Yakovleva, E.V. (1976). S t r e n g t h Mate
M e t a l l i c F i b e r s o f R e f r a c t o r y Meta l A l l o y s . " NASA CR-72654.
744-748.
4. Baranov, A.A. , and Yakovleva, E.V. (1975). S t r e n g t h Mater. 1, 966-969.
5. Ba r th , C . F . , B lake, D.W. , and Stetson, T.S. (1977). "Cost A n a l y s i s o f Advanced T u r b i n e Blade Manu fac tu r ing Processes." TRW-ER-17930, TRW Inc. , Cleveland, OH. ( A l s o , NASA CR-135203).
6. Baskey, R.H. (1967) . "F iber-Reinforced M e t a l l i c Composite M a t e r i a l s , " AFML-TR-67-196, A i r Force M a t e r i a l s Lab., Wr igh t P a t t e r s o n AFB, OH,
7 . B r e n t n a l l , W.D., (1976) . "Meta l M a t r i x Composites f o r High Temperature Tu rb ine Blades," TRW-ER-7790-F, TRW Inc., Cleveland, OH..(Also, NAOC-76225-30, Naval A i r Development Center) .
8. B r e n t n a l l , W.D., and Moracz, D.J. (1976). "Tungsten Wire-Nickel Base A l l o y Composite Development." TRW ER-7849, TRW Inc . , Cleveland, OH. ( A l s o , NASA CR-135021) .
9. B r e n t n a l l , W.D., and Toth, I .J. , (1974). " F a b r i c a t i o n o f Tungsten Wi re Re in fo rced Nlckel -Base A l l o y Composites." TRW-ER-7757, TRW Inc., Cleveland, OH. ( A l s o , NASA CR-134664).
10. B r e n t n a l l , W.D., Moracz, D.J., and Toth, I . J . (1975). "Meta l M a t r i x Composites f o r H igh Temperature Turbine Blades." TRW-ER-7722-F, TRW I n c . , Cleveland, OH.
11. C a u l f i e l d , T. (1986) . "Understanding t h e I n t e r d i f f u s i o n a l F lux Re la ted E f f e c t s on t h e H i g h Temperature C o m p a t i b i l i t y o f Tungsten F i b e r R e i n f o r c e d S u p e r a l l o y (TFRS) Composites." PhD Thesis, Columbia U n i v e r s i t y .
12. C a u l f i e l d , T., Be l lows, R.S., and Tien, J.K. (1985) . M e t a l l . Trans. A . l 6 , 1961 -1 968.
13. Chubarov, V. M., e t a l . (1972). S t reng th Mater. 3, 856-959.
14. Dean, A.V. (1965) . "The Reinforcement o f Nlckel-Base A l l o y s Wi th H i g h S t r e n g t h Tungsten Wires," NGTE-R-266, N a t i o n a l Gas Tu rb ine Es tab l i shmen t , Pystock, England.
1 5 . Dean, A .V . (1967) . J. I n s t . Met. 95, 79-86.
16. Dudnik, G . I . , Banas, F .P. , and Aleksandrov, B.V. (1973). S t r e n g t h Ma te r . - 5, 106-107.
1 7 . El-Dahshan, M.E., W h i t t l e , D.P., and S t r i n g e r , J . (1975) . Oxid. Met. 2, 45-67.
31
![Page 33: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/33.jpg)
18. tnd re5 , W. , (1974) . 'Hlgh-Temperature M a t e r l a l s i n Gas Tu rb lnes " ( P . R . Sahm and M. 0. Spe lde l , eds.) pp. 1-14. E l s e v i e r S c l e n t l f i c , New York.
19. F l e c k , J . N . (1979) . " F a b r l c a t i o n o f Tungsten-Wlre/FeCrAlY - M a t r l x Composltes Speclmens." TRW-ER-8076, TRW Inc . , Cleveland, OH.
20. Frledman, G . I . , and F leck , J.N. (1979) . "Tungsten Wire-Reinforced Supera l loys f o r 1093 " C (2000 O F ) T u r b i n e Blade A p p l i c a t l o n s . " TRW-ER-8135, TRW Inc. , Cleveland, OH. (A l so , NASA CR-159720).
21. Galduk, V . V . , Lavrenko, A.S., and Sukhanov, Yu. V . (1972). S t r e n g t h Mater . - 4, 1143-1146.
22. Garmong, G . (1974) . M e t a l l . Trans. 5, 2183-2205.
23. Glenny, R.J.E. (1970) . Proc. R. SOC. London A. m, 33-44.
24. Glenny, R.J.E., and Hopklns, B.E. (1976) . P h l l o s . Trans. R. SOC. London A. - 282, 105-118.
25. Gruenl lng, H., and Hofer , G. (1974). Z. W e r k s t o f f t e c h . 5, 69-72.
26. Hoffman, J . , Hofmann, S., and T i l lmann , L. (1974). Z. M e t a l l k d . 65, 721 -726.
27. Kannappan, A., and F i schme ls te r , H.F. (1975). "High Temperature M a t e r i a l s Phenomena" (M. T l l l i , ed.) Vol . 11, pp. 85-98. H e l s i n k i U n i v e r s i t y o f Technology, Esbo, F i n l a n d .
28. Karpinos, D.M., e t a l . (1972) . F l z . Khim. Obrab. Mater . 6, 107-113.
29. Karpinos, D.M., e t a l . (1975). Sov. Powder M e t a l l . Met. Ceram. (Eng l . Trans 1. ) 1 4 , 447-452.
30. K lng, G.W., (1972) . "Development o f Wlre-Drawing Processes f o r R e f r a c t o r y - Me ta l F l be rs . '' NASA CR-120925.
31. K l y p l n , B.A., Maslov, A.M., and Maslenkov, S.B., (1977). Met. S c i . Heat T rea t . Met. ( E n g l . T r a n s l . ) l9, 343-348.
32. Mazzel, P.J., Vandrunen, G., and Haklm, M.J. (1976) . "Advanced F a b r l c a t l o n Techniques i n Powder M e t a l l u r g y and T h e i r Economlc I m p l i c a t i o n s " AGARD-CP-200, AGARD, P a r i s , France.
33. Melnyk, P., and F leck , J.N. (1979). "Tungsten Wire/FeCrAlY M a t r l x T u r b i n e Blade F a b r i c a t i o n Study." TRW-ER-8101, TRW Inc . , Cleveland, OH. ( A l s o , NASA CR-159788).
34. M l r o t v o r s k l l , V.S., and O l ' s h e v s k l l , A.A. (1976). Sov. Powder M e t a l l . Met. Ceram. ( E n g l . T r a n s l . ) l5, 534-540.
35. M l r o t v o r s k i l , V.S., and O l ' s h e v s k i i , A.A. (1978). Sov. Powder M e t a l l . Met Ceram. (Eng l . T r a n s l . ) 17, 536-541.
32
![Page 34: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/34.jpg)
36. Mirotvorskli, V.S., and Ol'shevskll, A.A. (1979). Met. Sci. Heat Treat. Met. (Engl . Transl . ) 21, 826-829.
t
37. Montelbano, T., et al. (1968). Trans. Am. Inst. Min. Metall. Pet. Eng. - 242, 1973-1 979.
38. Morris, A.W.H., and Burwood-Smith, A. (1970). Fibre Sci. Technol. 3, 53-78.
39. Morrls, A.W.H., and Burwood-Smith, A . (1971). & "High Temperature Turbines" AGARD-CP-73-71, Paper 19. AGARD, Paris, France.
40. Nllsen, N., and Sovik, J.H. (1974). In "Practical Metallic Composites" pp. 851-854. Institution of Metallurglsts, London.
41. Ohnysty, B., and Stetson, A.R. (1967). "Evaluation of Composite Materials for Gas Turbine Engines." AFML-TR-66-156-Part-2.
42. Petrasek, D.W. (1972). "High-Temperature Strength of Refractory-Metal Wlres and Consideratlon for Composlte Applications." NASA TN D-6881.
43. Petrasek, D . W . , and Signorelli, R.A. (1969) "Stress-Rupture and Tensile Properties of Refractory-Metal Wlres at 2000 and 2200 O F (1093 and 204 "C) . I ' NASA TN 0-5139.
44. Petrasek, D.W., and Signorelli, R.A. (1970). "Preliminary Evaluation o f Tungsten Alloy Fiber - Nickel-Base Alloy Composites for Turbojet Engine Applications." NASA TN 0-5575.
45. Petrasek, D.W., and Signorelli, R.A. (1974). "Stress-Rupture Strength and Microstructural Stability of Tungsten-Hafnium-Carbon-Wire Reinforced Superalloy Composites." NASA TN D-7773.
46. Petrasek, D.W., and Weeton, J.W. (1963). "Alloying Effect on Tensile Properties and Micro-Structure of Tungsten-Fiber-Reinforced Composites." NASA TN D-1568.
47. Petrasek, D . W . , Slgnorelli, R.A., and Weeton, J.W. (1968). "Refractory- Metal-Fiber-Nickel-Base-Alloy Composltes for Use at High Temperatures." NASA TN 0-4787.
48. Petrasek, D . W . , et al. (1979). "Tungsten Fiber Reinforced FeCrAlY-A First Generatlon Composite Turbine Blade Material." NASA TM-79094.
49. Sahm, P.R. (1974). "High-Temperature Materials in Gas Turbines" (P.R. Sahm and M.O. Speidel, eds.) pp. 73-114. Elsevier Scientific, Amsterdam.
50. Severdenko, V.P., Matusevich, A.S., and Piskarev, A.E. (1974). Sov. Powder Metall. Met. Ceram. (Engl. Transl.) l3, 476-479.
51. Signorelli, R.A. (1972). "Review o f Status and Potential of Tungsten Wire: Superalloy Composites for Advanced Gas Turbine Engine Blades." NASA TM X-2599.
33
![Page 35: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/35.jpg)
52.
53.
54.
55.
56.
57.
58.
59.
Signorelli, H.A., Johnston, J.R., and Weeton, J.W. (1956). "Preliminary Investigation of Guy Alloy as a Turbojet-Engine Bucket Material for Use at 1650 O F . " NACA RM-E56119.
Speidel, M . O . (1974). In "High-Temperature Materials i n Gas Turbines" ( P . R . Sahm and M . O . Speidel, eds.) pp. 207-255. Elsevler Scientific, Ams t erdam . Stetson, A.R., et al. (1966). "Evaluation o f Composite Materials for Gas Turbine Engines." AFML-TR-66-156-Part-1, Air Force Materials Lab., Wright-Patterson AFB, OH.
Waters, W.J., Signorelli, R.A., and Johnston, J.R., (1959). "Performance of Two Boron-Modified S-816 Alloys in a Turbojet Engine Operated at 1650 O F . ' ' NASA Memo 3-3-59E.
Westfall, L.J. (1985). "Tungsten Fiber Reinforced Superalloy €omposite Monolayer Fabrication by an ARC-SPRAY Process." NASA TM-86917.
Winsa, E.A., and Petrasek, D.W. (1973). "Factors Affecting Miniature Izod Impact Strength of Tungsten-Fiber-Metal-Matrix Composites." NASA TN 0-7393.
Winsa, E.A., Westfall, L.J., and Petrasek, D.W. (1978). In "ICCM/2" (B.R. Norton et al, eds.) pp. 840-857. Metallurgical Society of AIME, Phi ladelphia.
Wukusick, C.S. (1966). "The Physical Metallurgy and Oxldation Behavior of Fe-Cr-A1-Y Alloys." GEMP-414, General Electrlc Co., Cincinnati, OH.
34
![Page 36: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/36.jpg)
TABLE I . - CHEMICAL C O M P O S I T I O N OF W I R E MATERIALS [42,43]
Mater i a1
Tungsten a l l o y s 218CS W-1T hO2 W-2Th02 W-3Re W-5Re-2Th02 W-24Re-2T h02
W-Re-Hf -C Tantalum a l l o y s
ASTAR 811C Molybdenum a l l o y s
TZM TZC
Niobium a l l o y s FS85 AS 30 B 88
W-Hf-C
- W
99.9 ba l
1 8.2
-___ ----
10.44 20 28.3
- Ta - Mo
Weight percent o f comDonent
Re T i Tho2 C
35
![Page 37: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/37.jpg)
TABLE 11. - REPRESENTATIVE PROPERTIES OF REFRACTORY-ALLOY WIRES [42,43]
A1 l o y s Density, Wire U l t i m a t e St ress f o r Stress/densi t ! gm/cm3 diameter, t e n s i l e 100-hr f o r 100-hr
mn s t r e n g t h r u p t u r e rup ture , cmxl03
k s i M N / d k s i MN/m2
-
126 14 2 173 214 176 211 207 314
108
113 125
66 61 77 -
I No. reac- t i o n
-
869 979
1193 1475 .213 ,455 1427 !165
745
779 862
455 421 531 -
I n t e r - m e t a l l i c compound
-
63 77 95 69 70 50
161 205
84
42 38
44 31 48 -
D i f f u - s i o n
penetra- t i o n
-
434 531 655 476 483 345
.110
.413
579
290 262
30 3 214 33 1 -
55 83 30
63 84 80
Tungsten a l l o y s 218CS W-lTh02
W-3Re W-5Re-2Th02 W-24Re-2T hop
W-Re-H f -C
W-2Th02
W-Hf-C
-- 12 --
-- --
3
234 282 356 249 254 183 584 744
351
295 267
19.1 19.1 18.9 19.4 19.1 19.4 19.4 19.4
16.9
10.0 10.0
10.5 9.7
10.2
0.20 .20 .38 .20 .20 .20 .38 .38
.51
.38
.13
.13
.13
.51
Tantalum a l l o y s ASTAR 811C
Molybdenum a1 l o y s TZM TZC
Niobium a l l o y s FS85 AS 30
295 224 328 888
6. 1204" (2200' F) Data
Tungsten a1 loys 218CS W-lTh02 W-2Th02 W-3Re W-5Re-2Th02 W-24Re-2T hop
W-Re-Hf-C Tantalum a l l o y s
ASTAR 811C Molybdenum a1 l o y s
TZM
W-Hf-C
19.1 19.1 18.9 19.4 19.1 19.4 19.4 19.4
16.9
10.0 10.0
10.5 9.7
10.2
0.20 .20 .38 .20 .20 .20 .36 .38
.51
.20
.13
.13
.13
.51
108 122 150 157 148 147 20 1 281
7 1
77 79
40 33 50
745 84 1
1034 1082 1020 1014 1386 1937
490
531 545
276 228 345
46 54 70 46 44 28
111 132
38
19 18
23
28 ---
31 7 372 483 317 30 3 193 765 910
262
131 124
159
193
170 198 257 168 160 102 404 480
157
135 127
155
190 ---
TZC
FS85 AS30 8 88
Niobium a l l o y s
TABLE 111. - COMPARISON OF FIBER-MATRIX REACTIONS FOR V A R I O U S
MATRIX MATERIALS r 3 6 i ~~~~ ~~
I R e l a t i v e no. o f cases. percent M a t r i x No. com- p o s i t i o n s
i n v e s t i- temper a t u r e
Recrys- t a l 1 iza-
t i o n
No. re - c r y s t a l - l i z a t i o n
gated
93 10
7 90 97
4 79 80
4 10 70
4 10 13
Ni-base 27 Co-base 29 Fe-base 30
Ni-base 27 Co-base 19 Fe-base 30
3
96 21 20
36
-
![Page 38: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/38.jpg)
TABLE I V . - PARABOLIC RATE CONSTANTS ( x 1O-l2crn2/s) FOR VARIOUS METAL
W-FIBER/MATRIX COMPOSITES ANNEALED
A T 1093 "C. K,(T) DENOTE THE OVERALL REACTION
ZONE KINETICS, THE F I B E R COMPONENT OF REACTION ZONE GROWTH, AND THE
MATRIX COMPONENT OF REACTION ZONE GROWTH, RESPECTIVELY
K,,(T), K f (T) , AND
[11,121
100 h r r u p t u r e s t r e n g t h
M N / d k s i ~
138 20
51 7.4 131 19
48 7 93 13.5
48 7 207 30
F e C r A l Y SS 316 I nco loy 907
Waspaloy .04
a A n n e a l e d a t 1100 "C.
Stress-densi ty f o r 100 h r r u p t u r e
m i n .
1125 44 300
635 25 000 1040 4 1 000
613 24 000 927 36 500
---- -__--- ---- _--__-
TABLE V. - RUPTURE STRENGTHS AN0 COMPOSITIONS FOR COMPOSITIES AN0 SUPERALLOYS
A. 100 h r r u p t u r e s t renqth a t 1100" C (2010' F) f o r composi t ies and supera l loys
23 138
193 324
Ref. 1 A1 l o y
3.3 254 10 000 1058 4 1 700 20
1513 59 600 2491 98 000
28 47
Wire
331 h r r u p t u r e strength-242 M N / d (35 k s i )
242 35
13 ZhS6 VRN tungsten
1 5 EPO-16 -_-------- 15 tungsten
38 Nimocast 713C ---------- 38 tunasten
1957 77 000
2147 84 500
_____-----
218CS (tungsten)
45 44 I W-29 h02 W-Hf-C
7 FeCrAlY W-l%Th02
Wire diam "01. % Densi ty
0.010
1.27 0.050 10.3
------- 9.15 0.33 0.38 0.015 40 13.3 .48
-_-____-_-- --
0.38 0.015 40 13.0 0.47 .38 .015 40 13.3 .48
0.38 1 0.015 I 56 112.5 1 0.45
20 FeCrAlY W-Hf-C 0.38 0.015 35 11.3 0.41
EPD-16 Nimocast 713C MARM322E Ni,Cr,W,Ti,Al
B. Nominal composit ion o f m a t r i x a l l o y s ( w e i g h t % )
Ni-12.5Cr-4.8Mo-7W-2.5Ti-5Al Ni-6A1-6Cr-2Mo-llW-1.5Nb Ni-12.5Cr-6Al-lTi-4M0-2Nb-2.5Fe Co-21.5C r-25 W-1ON i -0.8T i -3.5Ta Ni-15Cr-25W-2Ti-2Al Fe-24Cr-5A 1-1Y
37
![Page 39: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/39.jpg)
TABLE VI. - THERMAL CYCLING DATA FOR TUNGSTENlSUPERALLOY COMPOSITES - Ref. Remarks Composite material Heat source Cycle No. of
cycles
400 No apparent damage to interface
1 5
- 39
40 v/o WlNimocast 258 F 1 u id ized bed RT-1100' C (2010' F)
~~~~
Fluidized bed 2O0-6OO0 C (70'-1110' F) 550'-1050° C ( 102Oo-1~2O0 F) 20'-1050° C (70'-1920 F)
200 2-12 2-25
13 v/o W/Nimocast 713C No cracks Cracks at interface Cracks at interface
No. of cycles for fiber- matrix debonding 14 vlo - 90 to 100 cycles 24 v/o - 60 to 70 cycles 35 vlo - 35 to 50 cycles
16
- 3
- 8
- 10
W/EI435 (14, 24, and 35 v/o)
Electric resistance f urance
RT-1100' C (2010' F ) 2.5 min to temp. Water quench
100
W/EI435 (15 and 32 vlo)
Self resistance 30 sec to heat and cool 480°-7000 C (900°-12900 F) 30 sec to heat and cool 480°-7000 C (900°-12900 F) 50O0-8OO0 C (930°-1470' F ) 530'-900' C (980'-1650' F) 570°-1000' C( 105Oo-183O0 F) 600'-1100° C ( 1110°-2010" F)
1000 All 15 v/o specimens warped and had a speci- men length decrease. Cracks at interface. 35 v/o specimens did not deform externally but matrix cracks between fibers observed.
50O0-8OO0 C (930°-1470' F ) 530'-900' C (980'-1650' F) 570°-1000' C( 105Oo-183O0 F) 600'-1100° C ( 1110°-2010" F)
~~~
W /N i WCrA 1 Ti (35 and 50 vlo)
W / N i CrAl Y (35 and 50 vlo)
WI2IDA (35 and 50 v l o )
50 v/o W/NiCrAlY
Self resistance 1 min to heat 4 min to cool
RT-1093' C (2000' F)
100
100
100
1000
35 v/o warpage and shrinkage 50 vlo no damage
35 vlo warpage 50 v/o no damage
35 vlo warpage and shrinkage 50 v/o no damage
Internal microcracking
No damage Surface roughening but no crack i na
427'-1093' C ( 80O0-2O0O0 F ) ~~~
30 v/o W-l%Th02/FeCrAlY Passage of electric current
1 min to heat 4 min t o cool RT-1204' C f 2200" F)
1000
![Page 40: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/40.jpg)
3 0 0 r 2x103
200-
150-
1 0 0 -
50
250 L (u
E - iz f c3 z W E !Z W -1 * - I5 - - z c 5
-
0-
Figure 1.
0 I
z $ I
I
B
R N z c 0 1093OC F)
1204’ C 12200’ F)
TUNGSTEN BASE TANTALUM MOLYBDENUM NIOBIUM NICKEL BASE BASE BASE BASE
’ Ultimate tensile strength for refractory metal wires and superalloys. C42, 431
39
![Page 41: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/41.jpg)
16x103 6 x 1 6 r
b z w e
c i 3
0
+ e
U
0
e
3 d
& + v) W
v) z w c +
1 5 t 0 !
0 1093’ C (2oOo0 F) 0 1204’ C (22000 F)
V 4 A
I m
e
v) 2 a
TUNGSTEN BASE
TANTALUM MOLYBDENUM NIOBIUM NICKEL BASE BASE BASE BASE
Figure 2. - Ratio of ultimate tensi le s t rength to density fo r refractory metal wi res and superalloys. [42, 431
2 5 o r 1 6 x l d N E z - .-
VI Y
200 E m-
0” 12 I 8
% 8
z 150
L z z -
3 a
3 v) a 3 0 a
= 100 2 W v) w
2 5 0 , - 4 v)
w
v)
v) v) v) W
+ F & 8 t v)
V 4 A
I m
2 v) a
v, > s a --I
& W a 3 v)
n TUNGSTEN BASE TANTALUM MOLYBDENUM NIOBIUM NICKEL
BASE BASE BASE BASE
Figure 3. - Stress to cause rup tu re in 100 h o u r s fo r refractory metal wi res and superalloys. 1-42, 431
40
![Page 42: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/42.jpg)
8x 1 O3 m 1 0 3 r
,
cu z I- 4 I
3
N z c cu I
3 B
N z 2
t cu I
m I
3
V I r 3 I
n
0
L I - I
B I
3
m m
TANTALUM MOLYBDENUM NIOBIUM NICKEL BASE BASE BASE BASE
TUNGSTEN BASE
Figure 4. - Ratio of 100 hour rupture strength to density for refractory metal wires and superalloys. C42, 431
41
![Page 43: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/43.jpg)
Figure 5. - Recrystallization of tungsten f ibers in a copper plus 10 percent nickel matrix. C47]
42
![Page 44: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/44.jpg)
(a) Overall view.
\ \ L V A C U U M CHAMBER MATRIX
s POOL 7,
(b) Schematic of a r c spray process.
Figure 6. -Schematic view of a rc spray monotape fabrication unit.
43
![Page 45: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/45.jpg)
200
160 Y
s c3 z w
m w @=
120
z a 2 80 0: 3 0 I
5 4a
C
1200
600
400
200
218 CS TUNGSTEN
,I w-2% Tho2 -
FIBER
W-Hf -
w-2% 218 CS Th02 TUNG STEN
COMPOSITE
W-Hf-C
(FIBER - AS INDICATED MATRIX-Ni-15Cr-25W-2AI-2Ti)
Figure 7. - Comparison of 100 h o u r rup tu re strength at 1093' C 12O0O0 F) fo r f ibers and 70 volume percent f iber composites. C44, 45, 471
@= 3 0 I a A
40
10
a A
FI BER-TUN GSTEN MATRIX-NIMOCAST 258
mi-3.7Ti - 4.8 AI - 10 C r - 20 Co) 20
0 20 40 60 80 100 FIBER CONTENT, VOL. %
Figure 8 - Effect of f iber content on 100 h o u r composite rup tu re s t rength at llw C (20100 F). [151
4 4
![Page 46: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/46.jpg)
50 -
40- N E 1 E
30- g z W c4 I- v)
20- z L 3 c4 c4 2 10- g 8 .-(
0-
0 m A h
I- v)
0 0
z
a
z z 3 0 > - 0 N
\o
.- I- (u
NICKEL BASE
w
E p:
2
w N
s.4 E c4 - 2 N z
3
I-
N s
0 >
n COBALT IRON STRONGEST
BASE BASE SUPERALLOYS
Figure 9. - Comparison of 100 h o u r rup ture strength at 1099 C (2000' F) for composites and superalloys.
45
![Page 47: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/47.jpg)
loox lo? g v)
5 P E
E I- 60
80 n
c3
v) w p:
a 3
p: 3 0 L
? .!i
40
8 $ P
d
20
I-
0
-
V m d h
, MATRIX-
NICKEL BASE IRON BASE
i STRONGEST SUPERALLOYS
figure 10. - Comparison of t he rat io of 100 h o u r rup tu re strength t o density fo r composites and super- alloys at 1 0 9 9 c (2oooO F).
4 0 0 r
vi v) W
v) E
.- VI Y
MI v) W
v)
loo
40 100 400 1000
TIME TO RUPTURE, HOURS
Figure 11. - Stress versus t ime t o rup tu re comparison fo r composites and superalloys at 1099 C (2000' F).
46
![Page 48: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/48.jpg)
.- w l Y
In- v, W
v,
MATRIX- Ni-15Cr-25W- 2AI-2Ti
1 100 400 1000
TIME TO RUPTURE, HOURS
Figure 12. - Stress (tocause rup tu re ) to density rat io for com- posites and superalloys at 1093' C (2000° F).
30
20
10
N E z E - vi v, W E + v,
RANGE FOR TFRS 40 vlo FIBER AT 20@ F
0 1500 1600 1700 1800 1900 2ChM
0 L TEMPERATURE, O F
800 900 1000 1100 TEMPERATURE, OC
Figure 13. -Comparison of 100 h o u r rup tu re strength for TFRS and superalloys.
47
![Page 49: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/49.jpg)
200x103 5x103 r I-
c E1' 150 ai c - z
0" 100 2
v, z
E c3 2 I- z 50/
v,
RANGE
SUPER- ALLOYS
wl
n
0, 2 c WA FOR TFRS 40 vlo FIBER
AT 2ooo0 F
I 1 1 I I 1500 1600 1700 1800 1900 2000
TEMPERATURE, O F
OL
L 800 900 lo00 1100
TEMPERATURF, O C
Figure 14. - Comparison of the rat io of 100 h o u r rup tu re strength to den- sity for TFRS and superalloys.
z 0
a z E c
W
2.0
Q 1.5
1.0
-
ln I- ii I 713 C 140 M N l d
.5
0 10 20 30 40 50 60 70 80 TIME, HOUR
Figure 15. - Cornparison of typical creep behaviour of Nimocast 713C wi th and wi thout tungsten reinforce- ment at ll@ c (20100 F). ~381
48
![Page 50: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/50.jpg)
80
40 v)
L I
L
I 1 I
0 HASTELLOYX COMPOSITE HASTELLOY X- W-1 %Tho2 WIRE
35 d o
23 vlo 36 VI0
816O C 9000 c 982' C TEMPERATURE (1500' F) (16500 F) (18000 F)
TEMPERATURE
Figure 16. - Stress fo r failure in 1x106 cycles for Hastelloy X and composite. C61
W-1%Th02 WIRE/
49
![Page 51: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/51.jpg)
d 1 I 105 106 107 108
L NO. OF CYCLES TO FAILURE
Figure 18 - Stress as a funct ion of number of cycles to fa i lu re for W-l%Th021 FeCrAlY composites tested at 7600 C (14000 F). [191
0 3 5 V D 40
A > 20 - A Ls 0-
A I
NO. CYCLES TO FAILURE
Figure 19. - Stress as a func t i on of number of cycles to fa i lu re fo r W-l%ThO$ FeCrAlY composites tested at C (19000 F). [19]
" '/,',\ Y Y X I
I' ' IINIMONIC 75 '~NIMONIC 95 'NlOMlC 105 A
3
n I I " 1400 1600 1800 2000
I I i I 700 800 900 lo00 1100
TEMPERATURE, OF
TEMPERATURE, OC
I
Figure 20. - High-cycle fatigue s t rength rat io comparison for TFRS and superalloys.
50
![Page 52: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/52.jpg)
0 100 pm W in Ni, Liq. inf. v 300pm W in Ni. sinter-forged 0 500pm W in Ni, Liq. inf.
. 4 103 104 Id 106
NUMBER OF CYCLES TO FAILURE
Figure 21. - Ratio of fatigue s t rength (aF) to ult imate tensi le strength (UTS) for Ni/W cont inuously re in - forced composites. [403
VOLUME, percent, FIBER TEST TEMPERATURE 0 35 7600 C (1406' F) 0 35 9800 C (1806' F) a 20 7600 C (1406' F) 0 20 9800 C (1806' F)
2 0 0 L
90 r
40 I- - L!r-
20 " 1 101 102 103 104
CYCLES TO FAILURE
Figure 22. - Maximum stress versus cycles t o fa i lure fo r W-l%ThOz/ FeCrAlY com- posites. L191
![Page 53: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/53.jpg)
a 20 7600 C (14000 F) 0 35 7600 C (14000 F) 0 20 9800 C (18000 F) 0 35 9800 C (18000 F)
1. O r
- 8 t I
101 102 103 18 CYCLES
Figure 23. - Ratio of fatigue strength t o ult imate tensi le strength versus cycles t o fai l- u r e for W- l%Th02/ FeCrAlY composites. [19]
- v - .v-- -
1000 CYCLES 3OO-120OO C (85O-22oOO F)
Figure 24. - Photomicrographs of the r - mally cycled tungsten w i r e reinforced FeCrAlY composite. (Photos courtesy of I rv ing Machlin). [81
52
![Page 54: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/54.jpg)
TEMPERATURE, OC (OF)
0 24(75) W 538(1000)
(a) UNNOTCHED. W
In e 3
“t 20 ;k rd’ , , // 0
0 10 20 30 40 50 60 70 80 FIBER CONTENT, VOLUME, PERCENT
(b) NOTCHED
Figure 25. - Impact strength of unnotched and notched as- HIP tungstenlsuperalloy as a function of fiber content. C571
53
![Page 55: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/55.jpg)
i c3 z W 01 I- v) I- V a n z
80
20 I' t c3 z W & I- v)
lor FIBER CONTENT, VOLUME, PERCENT
:t 4 [-- 2 -1 L -<
L 0 L L a n 3
20
4 6l (a) UNNOTCHED.
I / 40 2 c / /
0 0
100 500 700
l- Or TUNGSTENISUPERALLOY.
0 L
54
![Page 56: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/56.jpg)
W & t- v)
t-
I- v) a
z
_c_
TESTED AT TESTED AT 24' C (700 F) 7600 C (1406' F)
Figure 28. - Min ia tu re lzod impact strengths of unnotched tung stenlnickel-base superalloys compared to m i n i m um impact strength standard used to screen potential t u rb ine blade and vane materials. [571
CLADDING
TEST CONDITION - EXPOSED TO AIR ATMOSPHERE FOR 50 HR AT 1093 OC (2000 OF)
Figure 29. - Transverse section of oxidized refractory f iber - nickel alloy composite. L443
55
![Page 57: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/57.jpg)
OXIDATION I N LONGITUDINAL DIRECTION CONTINUOUS PATH FOR OXIDATION OF FIBER
(OXIDATION I N TRANSVERSE DIRECTION EXPOSED SURFACE FIBERS OXIDIZE NEXT ROW OF FIBERS PROTECTED FROM OXIDATION BY LAYER OF MATRIX
Figure 30. - Pr inc ipa l paths f o r exposed f iber oxidation.
65 v lo WlALLOY 3 OAA 2 ' LONGITUDINAL
w
10
50 v lo WlFeCrAlY - 8 ..TRANSVERSE
P 04
'-ALLOY 3 0-
100 300 500 700 900 TEMP, OC u
200 600 1000 1400 TEMP. OF
Figure 31. - Measured ther - mal conductivi ty of TFRS composites and matr ix al- loys. 1581
56
![Page 58: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/58.jpg)
WIFeLrAIY IMPINGEMENT COOLING INSERT
I
LROOT HALVES BRAZED OR DIFFUSION BONDED TO AIRFOIL OR ROOT FABRICATED FROM PLIES OF WISUPERALLOY & SUPERALLOY TO GIVE GRADED THERMAL EXPANSION
Figure 32. - Schematic of FRS JT9D blade designed fo r fabrication feasibility expe r i in en t s.
WlFeC
‘STEEL TO BE LEACHED
WlFeC
‘STEEL TO BE LEACHED
LEADING EDGE CORE
Figure 33. - Schematic of airfoil p ly configuration in JT9D blade.
57
![Page 59: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/59.jpg)
~ E R AND MATRIX SHEETS
MONOTA P E DIE CUT PLIES
NEAR NET SHAPE Figure 34 - TFRS blade fabrication process.
58
![Page 60: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/60.jpg)
ORIGINAL PAGE \S OF POOR QUALITY
Figure 35. - Composite hollow airfoil.
Figure 36. - Hollw composite blade.
59
![Page 61: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/61.jpg)
Figure 37. - Tungsten fiberlsuperalloy composite blade.
ORIGJNRL PAGE tS W POOR QUALITY
CYIELD 54%
- D SE 37%
FINAL ACCEPTANCE ._ __ COATING - --MACHININGIFINI SHlNG
FA 6 RIC A l l ON
ODs -t y'
67% W + FeCrAlY
53%
Figure 38. - Cost analysis for JT9D first stage turbine blade. C5l
60
![Page 62: Fiber Reinforced Superalloys - NASA · PDF file · 2013-08-30FIBER REINfORCED SUPERALLOYS Donald W. Petrasek and Robert A. Signore111 National Aeronautics and Space Administration](https://reader031.vdocuments.site/reader031/viewer/2022030505/5ab2dfff7f8b9ac66c8db70f/html5/thumbnails/62.jpg)
1. Report No.
NASA TM-89865
Fiber Reinforced Superalloys
2. Government Accession No. 3. Reclplent's Catalog No.
April 1987
505-63-81 7. Author@) 8. Performlng Organlzation Report No.
Donald W . Petrasek, Robert A . Signorelli, Thomas Caulfield, and John K . Tien
7. Key Words (Suggested by Author@))
Composites; High temperature material; Tungsten alloy fibers; High strength matertal; Superalloy; Turbine engine mater i a 1
I E-3533
18. Olstrlbutlon Statement
Unclassified - unlimited STAR Category 24
10. Work Unlt No.
9. Security Classif. (of this report) 20. Security Classif. (of thls page) 21. No. of pages Unclassifled Unclassified 61
9. Performing Organlzation Name and Address 11. Contract or Grant No.
National Aeronautics and Space Administration
22. Price' A04
Lewis Research Center Cleveland, Ohio 44135 13. Type of Report and Period Covered
2. Sponsoring Agency Name and Address 1 Technical Memorandum National Aeronautics and Space Administratjon Washington, D.C. 20546
14. Sponsorlng Agency Code I 5. Supplementary Notes
Donald W . Petrasek and Robert A. Signorelli, NASA Lewis Research Center, Thomas Caulfield and John K . Tien, Columbia University, New York, New York 10027. Proposed Chapter of Superalloys, Composites, and Ceramics published by Academic Press Inc.
Improved performance of heat engines i s largely dependent upon maximum cycle tem- peratures. family of high temperature composites that offer the potential for significantly raising hot component operating temperatures and thus leading to improved heat engine performance. This status review of TFRS research emphasizes the promising property data developed to date, the status of TFRS composite airfoil fabrication technology, and the areas requiring more attention to assure their appllcabillty to hot section components of aircraft gas-turbine engines.
6. Abstract
Tungsten fiber reinforced superalloys (TFRS) are the first of a