C.A. Yablinsky, M.J. Mills, K.M. Flores, J.C. Williams
Joe Rigney- GE
MEANS2 Meeting
Fatigue Behavior in Ni-base Superalloys for blade applications
![Page 2: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/2.jpg)
2
Introduction- Modern Designs
• Modern designs have cooling channels. • Experience and experimental studies show
fatigue is the life-limiting factor
![Page 3: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/3.jpg)
3
Introduction: Turbine blade fatigue• Sources of Fatigue:
– Mechanical stress due to centrifugal motion and stress concentrations
– Thermal-mechanical fatigue (TMF) due to local hot spots constrained by cooler surrounding regions
• Isothermal Sustained Peak Low Cycle Fatigue (SPLCF) Tests:– Mimic TMF cycles and behavior– Each cycle has hold time
• Comprehensive fatigue mechanism investigations have not previously been done
High Temperature
Low Temperature
Temperatures within an airfoil
![Page 4: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/4.jpg)
4
Experimental Details• Material
– Monocrystalline Ni-based superalloy René N5– Coated, cylindrical specimens
• Sustained Peak Low Cycle Fatigue Testing– Temperature: 980°C-1090°C– Total Strain Control– Held in compression or tension
Ni Cr Co Mo W Al5 6.2
Ta Re7 3
Hf61.8 7 8 2 0.2
Durand-Charre, Madeleine. The Microstructure of Superalloys.Amsterdam: Gordon and Breach Science, 1997. p11.
![Page 5: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/5.jpg)
5
Stress State Changes in SPLCF CyclesCompression Hold• Yield possible, creep relaxation• Mean stress shift upward• Positive mean stress develops
Tension Hold• Creep relaxation• Mean stress shifts down
(+)
σ
(+)
(-)
1st cycle 2nd cycle 3rd cycle
t
tε
(-)
σ
(+)
(-)
1st cycle 2nd cycle 3rd cycle
t
t
ε
(-)
(+)
![Page 6: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/6.jpg)
6
2mm 2mm2mm
SEM Fractography- Compression
• Crack initiation at surface• Multiple initiation sites• Crack propagation depends on temperature
– Environmental effects
1090°C 980°C 1040°C
Primary Initiation SitesSecondary Initiation Sites
![Page 7: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/7.jpg)
7
SEM Fractography- 1040°C, 0.9%
• Striations• Change in crack plane• Surface is oxidized along
crack wake
2mm2mm
Compression hold Tension hold
• Creep deformation observed; initiating at casting pores and carbides
• Macroscopically flat fracture surface
![Page 8: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/8.jpg)
8
SEM γ’ Characterization- 1040°C
• Cuboidal γ’• No preferential alignment (no rafting)• Note: γ phase is the lighter phase in all pictures
Thermally Exposed Material- No StressParallel Transverse
5μm 5μm
![Page 9: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/9.jpg)
9
SEM γ’ Characterization- 1040°C, 0.9%
• N-type– Rafted perpendicular to tensile
loading direction• γ phase shorter than seen in
creep alone
• P-type – Rafted parallel to tensile
loading direction• Rafted domains in
orthogonal orientation
Compression hold Tension holdParallel Transverse Parallel Transverse
γ’ phase is continuous phaseThese types of rafted structures are seen for negative misfit
5μm 5μm
![Page 10: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/10.jpg)
10
TEM- Thermally Exposed Material- 1040°C
• Dislocations at γ/γ’interface
• Dislocation looping around γ’ phase
g020
500nm
![Page 11: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/11.jpg)
11
SPLCF Results- 1040°C, Compression hold
• Extensive dislocation networks in γ and at γ/γ’ interfaces
• Dislocations in γ’
γ
γγ’
g020
g200
500nm200nm
![Page 12: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/12.jpg)
12
500nm
γ’
γ
g200
3au
SPLCF Results- 1040°C, Tension hold• Dislocation network in γ
phase and at γ/γ’ interface• 001 superdislocations in γ’
phase
g020
200nm
![Page 13: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/13.jpg)
13
Conclusions• Fracture is very different
– Compression hold• Crack propagation from surface• Oxidation of fracture surface in crack wake
– Tension hold• Crack propagation from casting pores• Surface macroscopically flat
• Rafted microstructure from cuboidal structure under stress
• P-type rafting with compression hold• N-type rafting with tension hold
– Broken microstructure due to influence of fatigue compared to rafted creep structures
![Page 14: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/14.jpg)
14
Conclusions- cont.• TEM
– Thermally exposed• Dislocations along γ/γ’ interfaces, which have begun
looping around γ’ phase– Compression hold
• Extensive dislocation networks in γ• Dislocations in γ’
– Tension hold• Dislocation networks at γ/γ’ interfaces; • 001 superdislocations in γ’
![Page 15: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/15.jpg)
15
Future Test Plans
• Test cylindrical specimens under low cycle fatigue conditions in order to study deformation mechanisms that lead to damage accumulation and crack initiation.
–Use the FIB/TEM technique to examine deformation at the initiation site
–Determine the crystallography of the initiation site
–Determine the crystallographic plane(s) of crack propagation
• Existing LCF and SPLCF samples (Coated)–New tests on uncoated specimens in air
![Page 16: Fatigue Behavior in Ni-base Superalloys for blade](https://reader030.vdocuments.site/reader030/viewer/2022012614/619a7ac753c4755e7f02e97a/html5/thumbnails/16.jpg)
16
Future Test Plans
• Test compact tension specimens under cyclic loading conditions to determine the influence of microstructure on crack propagation and fatigue failure. – Test effects of load ratio, environment, and
crystallographic orientation– Use the FIB/TEM technique to examine deformation in
the plastic zone ahead of the crack tip and in wake of the crack.
• Analyze and compare deformation mechanisms at the crack initiation site, ahead of the crack tip, in the plastic wake of the crack, and in the bulk material.
• Compare results to SPLCF results.