experimental study on the damage evolution of re-bar concrete interface lu xinzheng sce, thu cse,...
Post on 23-Jan-2016
220 views
TRANSCRIPT
![Page 1: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/1.jpg)
Experimental Study on the Damage Evolution of Re-bar Concrete Interface
Lu Xinzheng
SCE, THU CSE, NTU
1999/2000
![Page 2: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/2.jpg)
Abstract
A new type of bond-slip test is developed in this study
Constitutive relationship of bond is obtained for the test
FEA using this constitutive relationship Result analysis and comparing
![Page 3: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/3.jpg)
General Overview
Introduction and Literature Review Experiment Procedure Experimental Data Analysis Numerical Computation Study Conclusion and Discussion
![Page 4: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/4.jpg)
1.1 Introduction
00
00
0~
iiii
iiiiii and
orwhen
DD
• Liu Yu’s Concrete Model
3
2
1
~
~
~
~
D
D
D
D
(a). (b). (c). (d).
![Page 5: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/5.jpg)
RCED Model (RC Element Damage Model)
Damage in the reinforced concrete
1. Effective damage in concrete
2. Slip between concrete and re-bar
3. Local damage in concrete due to slip
![Page 6: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/6.jpg)
RCED Model (RC Element Damage Model)
F
Local damage
x
l
Affected zone
Local damage zone in RCED Model
![Page 7: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/7.jpg)
RCED Model (RC Element Damage Model)
o
z
y
x
87
6
5
4
3
21
10,12
9,11
Element in RCED Model
![Page 8: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/8.jpg)
1.2 Literature Review
Bond Test Method
1. Pull-out Test
2. Beam-type Test
3. Uniaxial-tension Test
![Page 9: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/9.jpg)
Pull-out Test
Figure 1.5 no-transverse bar withdrawing test Figure 1.6 with transverse bar withdrawing testNo-transverse bar pull-out test With transverse bar pull-out test
![Page 10: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/10.jpg)
Pull-out Test
hoop rebar
Plastic Pipe Eccentric Rebar Central Rebar
Figure 1.7 Specimen With Hoop Rebar Specimen with Hoop Rebar
![Page 11: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/11.jpg)
Pull-out Test
Plastic Pipe
Web Rebar
Bonding Area
Figure 1.8 Specimen With Web Rebar Specimen with Web Rebar
![Page 12: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/12.jpg)
Pull-out Test
Plasitc Pipe
Figure 1.9 Rebar In Different Place Rebar in Different places
![Page 13: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/13.jpg)
Feature of Pull-out Test
Strongpoint
1. Can determine the anchoring strength of bond
2. Easy to procedure
Shortage
Complex stress state around the surface
![Page 14: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/14.jpg)
Beam-type Test
Plasitc Pipe
Figure 1.10 Half Beam Test to Simulate the Inclined Crack
Figure 1.11 Half Beam Test to Simulate the Vertical Crack Half-beam Test to
Simulate the Inclined Crack
Half-beam Test to Simulate the Vertical
Crack
![Page 15: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/15.jpg)
Beam-type Test
Figure 1.12 Full Beam Test to Simulate the Vertical Crack
Figure 1.13 Full Beam Test to Simulate the Inclined Crack
Half-beam Test to Simulate the Inclined Crack
Half-beam Test to Simulate the Vertical Crack
![Page 16: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/16.jpg)
Beam-type Test
3 2 1
Figure 1.14 Simple Supported Beam Test
1: Lever-type Strain Gauge 2: Stain Gauge On the Bottom 3: Strain Gauge on the Side
Simply Supported Beam Test
1: Lever-type Strain Gauge 2: Strain Gauge On the Bottom3: Strain Gauge on the Side
![Page 17: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/17.jpg)
Feature of Beam-type Test
Strongpoint
1. Very close to the real state
2. Can determine bond strength of both
anchoring zone and between cracks Shortage
Complex and Expensive
![Page 18: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/18.jpg)
Uniaxial-tension Test
Figure 1.15 Uniaxial-draw TestUniaxial-tension Test
![Page 19: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/19.jpg)
Feature of Uniaxial-tension Test
Strongpoint
1. Can determine the bond stress between cracks
2. Easy to Procedure
Shortage
Complex distribution of bond stress
![Page 20: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/20.jpg)
2. Procedure of Test
1. Assumption in RCED Model
a. Pure shear deformation in the bond zone
b. Linear slip field
2. Test purpose
a. Determine the evolution of Ds
b. Determine the rational size of RCED element
c. Determine the parameter of a1, a2
![Page 21: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/21.jpg)
Test Device and Method
210
mm
75 m
m
15m
m
RConcrete
Steel Bar
Figure 2.2 Specimen
RC Specimen
![Page 22: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/22.jpg)
Test Device and Method
Clamping Device
LVDT 5
LVDT 4
LVDT 9
LVDT 2,3
LVDT 6,7
LVDT 8
Steel Plate
Figure 2.3 Load Apply Device
Loading Device
![Page 23: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/23.jpg)
Test Device and Method
Steel Bar
PVC PipePVC Pipe
Concrete
Figure 2.4 The Stress State of SpecimenStress State of the Specimen
![Page 24: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/24.jpg)
Test Device and Method Assumption in RCED
Model
1. Shear deformation in bond zone
2. Linear slip field
Feature of the Test
1. Constraint force is applied through PVC pipe and glue. Concrete is under pure shear stress condition
2. Specimen is as thin as possible
Conclusion: This test can satisfy RCED model
![Page 25: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/25.jpg)
Test Device and Method
(a) Concrete Specimen
before Test
(b) PVC Pipe before Test
![Page 26: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/26.jpg)
Test Device and Method
(c, d) During the Test
![Page 27: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/27.jpg)
Test Device and Method
Test Device Setup
![Page 28: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/28.jpg)
Test Procedure
Design the Mold Test of Steel Bar Casting of Concrete Design of Loading Device Specimen Analysis before Test Trial Loading and Analysis of Failure Improving Method Formal Loading Standard Specimen Test
![Page 29: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/29.jpg)
1. Design the Mold
Round Poly-
wood Plate
Steel Bar
PVC Pipe
Poly-wood PlateGlue
Specimen Mold
![Page 30: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/30.jpg)
2. Test of Steel Bar
Displacement Determined By LVDT 5
Slip Between Steel Bar and Concrete
Elongation of the Free Part of Steel Bar
Slip Between Steel Bar and Clamping Device
![Page 31: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/31.jpg)
2. Test of Steel Bar
Clamping Device
LDVT
Steel Bar
![Page 32: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/32.jpg)
2. Test of Steel Bar
0
100
200
300
400
500
600
700
0 0. 02 0. 04 0. 06 0. 08 0. 1 0. 12 0. 14
Strai n
Str
ess
(M
Pa)
Bar1Bar2Bar3
![Page 33: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/33.jpg)
2. Test of Steel Bar
y = 65948x + 18. 185
0
50
100
150
200
250
300
350
400
450
0 0. 001 0. 002 0. 003 0. 004 0. 005 0. 006
Strai n
Str
ess
(M
Pa)
![Page 34: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/34.jpg)
5. Specimen Analysis before Test
0
2
4
6
8
10
12
14
21 21. 5 22 22. 5 23 23. 5 24 24. 5 25 25. 5 26 26. 5
Ti me (mi l i second)
Test
Nu
mb
er
![Page 35: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/35.jpg)
6. Trial Loading and Analysis of Failure
Concrete Fail Surface
Steel Plate
Fail Surface of 10-7
![Page 36: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/36.jpg)
6. Trial Loading and Analysis of Failure
Test Result of 10-7
![Page 37: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/37.jpg)
6. Trial Loading and Analysis of Failure
Clamping Device
LVDT 5
LVDT 4
LVDT 9
LVDT 2,3
LVDT 6,7
LVDT 8
Steel Plate
Load Applied directly without PVC Pipe
![Page 38: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/38.jpg)
6. Trial Loading and Analysis of Failure
Load Applied directly without PVC Pipe
![Page 39: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/39.jpg)
6. Trial Loading and Analysis of Failure
Conclusion obtained from trial loading
1. The adhesive isn’t process properly
2. The confinement is still large
![Page 40: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/40.jpg)
7. Improving the Method
Roughen the adhesive interface deeper Split the PVC pipe finely
![Page 41: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/41.jpg)
8. Formal Loading
Test Result of 10-1
![Page 42: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/42.jpg)
8. Formal Loading
Test Result of 15-5
![Page 43: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/43.jpg)
8. Formal Loading
Test Result of 10-5
![Page 44: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/44.jpg)
8. Formal Loading
Test Result of 10-4
![Page 45: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/45.jpg)
8. Formal Loading
Test Result of 15-1
![Page 46: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/46.jpg)
8. Formal Loading
Test Result of 15-6
![Page 47: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/47.jpg)
8. Formal Loading
Test Result of 20-1
![Page 48: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/48.jpg)
8. Formal Loading
Test Result of 20-5
![Page 49: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/49.jpg)
9. Standard Specimen Test
Standard Tube Specimen• Size: 15×15×15cm
• Result:
Specimen Number 1 2 3
Max Load (KN) 953 1061 959
Max Strength (MPa) 42.36 47.16 42.62
![Page 50: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/50.jpg)
9. Standard Specimen Test
Strain Gauge
Six Strain Gauges on Standard Cylinder Specimen
![Page 51: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/51.jpg)
9. Standard Specimen TestStress-Strai n
0
5
10
15
20
25
30
35
-2000 0 2000 4000 6000 8000 10000 12000
Strai n
Str
ess
(M
Pa)
Cyl i nder1 Cyl i nder2 Cyl i nder3
Lognitudinal-stress-strain Curve
![Page 52: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/52.jpg)
9. Standard Specimen Testσ 3-ε 2, ε 3
0
0. 2
0. 4
0. 6
0. 8
1
1. 2
0 1000 2000 3000 4000 5000 6000 7000 8000 9000 10000
ε 2, 3
σ3/f
c
Cyl i nder1 Cyl i nder2 Cyl i nder3
Side-stress-strain Curve
![Page 53: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/53.jpg)
9. Standard Specimen TestPoi sson Factor
0
0. 2
0. 4
0. 6
0. 8
1
1. 2
0 0. 5 1 1. 5 2 2. 5
Poi sson Factor
σ3
/fc
Cyl i nder1 Cyl i nder2 Cyl i nder3
Stress- Poisson Ratio
![Page 54: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/54.jpg)
3. Experimental Data AnalysisLoad-Di spl acement of 10-5
-5
0
5
10
15
20
25
-6 -5 -4 -3 -2 -1 0 1
di spl acement (mm)
Load
(K
N)
TopCenter1 TopCenter2 TopEdge TopST
Topical Experiment Original Data
![Page 55: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/55.jpg)
3. Experimental Data Analysis
The following information can be obtained from the experimental data:
1. -1+2 Curve 2. Influence of Height and Radius of Specimen3. Shear Stress Distribution of Steel Bar and Deformation of Concrete4. Slip Damage Zone
![Page 56: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/56.jpg)
Original Data
Load-Di spl acement of 10-5
-5
0
5
10
15
20
25
-6 -5 -4 -3 -2 -1 0 1
di spl acement (mm)
Load
(K
N)
TopCenter1 TopCenter2 TopEdge TopST
![Page 57: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/57.jpg)
-1+2 CurveStress-Δ 1+Δ 2
-2
0
2
4
6
8
10
12
-2 0 2 4 6 8 10
Δ 1+Δ 2 (mm)
Str
ess
(M
Pa)
10-1 10-2 10-3 10-4 10-5 10-6
![Page 58: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/58.jpg)
-1+2 CurveStress-Δ 1+Δ 2
-2
0
2
4
6
8
10
-2 0 2 4 6 8 10 12
Δ 1+Δ 2 (mm)
Str
ess
(M
Pa)
15-1 15-2 15-3 15-4 15-5 15-6 15-7
![Page 59: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/59.jpg)
-1+2 CurveStress-Δ 1+Δ 2
-2
0
2
4
6
8
10
12
-2 0 2 4 6 8 10
Δ 1+Δ 2 (mm)
Str
ess
(M
Pa)
20-1 20-2 20-3 20-5 20-6 20-7
![Page 60: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/60.jpg)
-1+2 CurveStress-Δ 1+Δ 2
-2
0
2
4
6
8
10
12
-2 0 2 4 6 8 10
Δ 1+Δ 2 (mm)
Str
ess
(M
Pa)
30-1 30-2 30-3 30-4 30-5
![Page 61: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/61.jpg)
-1+2 Curve FittingStress-Δ 1+Δ 2
-2
0
2
4
6
8
10
12
-2 0 2 4 6 8 10 12
Δ 1+Δ 2 (mm)
Str
ess
(M
Pa)
10-1 10-2 10-3 10-4 10-5 10-6 fi tti ng
![Page 62: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/62.jpg)
-1+2 Curve FittingStress-Δ 1+Δ 2
-2
0
2
4
6
8
10
-2 0 2 4 6 8 10 12
Δ 1+Δ 2 (mm)
Str
ess
(M
Pa)
15-1 15-2 15-3 15-4 15-5 15-6 15-7 Fi tt i ng
![Page 63: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/63.jpg)
Empirical Formula
87.2
00
2.3
00max
)(642.0)(916.01
)(061.0)(7260.0
, Average bond stress
, Value of 1+2
0, Value of 1+2 at peak point
![Page 64: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/64.jpg)
Influence of Height of SpecimenStrength to Hei ght
0
2
4
6
8
10
12
74 76 78 80 82 84 86 88 90
Hei ght (mm)
Sh
ear
Str
en
gth
(M
Pa)
Ave Strength to Hei ght Fi tt i ng for Strenth-Hei ght
![Page 65: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/65.jpg)
Influence of Radius of Specimen
Strength to Radi us
0
2
4
6
8
10
12
0 5 10 15 20 25 30 35
Radi us(mm)
Str
en
gth
(MPa
)
Strength Average Strength
![Page 66: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/66.jpg)
Shear Stress Distribution along Steel Bar Obtain the Shear Stress Distribution from
the following conditions
1. Elongation of the steel bar
2. Relationship between and 3. Linear assumption in RCED model
![Page 67: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/67.jpg)
Shear Stress Distribution along the Steel Bar
Steel Bar Shear Stress Tmi n/ Tmax(Load Peak Poi nt)
0
0. 1
0. 2
0. 3
0. 4
0. 5
0. 6
0. 7
0. 8
0. 9
1
0 5 10 15 20
Tm
in/T
max(L
oad
Peak P
oin
t)
Stress Rati oAverage
![Page 68: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/68.jpg)
Slip Damage Zone
In this test, there is no obvious slip damage zone founded with UPV. So we consider that the slip damage zone is very small, which appears just around the interface of concrete and re-bar.
![Page 69: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/69.jpg)
Numerical Study
Objectives
1. Whether the empirical relationship of bond-slip obtained from the test can be used directly in finite element analysis
2. To verify the assumption in RCED model
![Page 70: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/70.jpg)
Numerical Study
Finite Element Analysis Software
1. Linear analysis: MARC k 7.3.2
2. Non-linear analysis: Sap 91 Element Type and Mesh
Concrete, Steel bar, Glue and PVC pipe: 20 nodes 3D element.
Bond: Spring element
![Page 71: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/71.jpg)
Mesh of Specimen Series 10
![Page 72: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/72.jpg)
Mesh of Specimen Series 15
![Page 73: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/73.jpg)
Numerical Result
![Page 74: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/74.jpg)
Comparison with Test ResultsResul t of Test and FEA(Stress-Δ 1+Δ 2), Speci men Seri es 10
-2
0
2
4
6
8
10
12
-0. 2 0 0. 2 0. 4 0. 6 0. 8 1 1. 2 1. 4
Δ 1+Δ 2 (mm)
Sh
ear
Str
ess
(M
Pa)
Test Poi nt Li near FEA Non- l i near FEA Fi tt i ng for Test Poi nt
![Page 75: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/75.jpg)
Comparison with Test ResultResul t of Test and FEA(Stress-Δ 1+Δ 2), Speci men Seri es 15
-2
0
2
4
6
8
10
12
0 0. 2 0. 4 0. 6 0. 8 1 1. 2 1. 4 1. 6 1. 8
Δ 1+Δ 2 (mm)
Sh
ear
Str
ess
(M
Pa)
Test Poi nt Li near FEA Non-Li near FEA Fi tt i ng for Test Poi nt
![Page 76: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/76.jpg)
Comparison with Test ResultStress-Deformati on of Concrete 10
0
2
4
6
8
10
12
0 0. 05 0. 1 0. 15 0. 2 0. 25
Deformati on (mm)
Str
ess
(M
Pa)
Test Poi nt FEA Li near Resul t FEA Non-Li near Resul t Fi tt i ng to Test Poi nt
![Page 77: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/77.jpg)
Comparison with Test ResultStress-Deformati on of Concrete (15)
0
2
4
6
8
10
12
0 0. 05 0. 1 0. 15 0. 2 0. 25Deformati on (mm)
Str
ess
(M
Pa)
Test Poi nt FEA Li near Resul t FEA Non-Li near Resul t Fi tt i ng to Test Poi nt
![Page 78: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/78.jpg)
Comparison with Test Result
The errors between the test results and numerical results are smaller than 10%.
Hence, the bond-slip relationship obtained from the test can be directly used in finite element analysis.
![Page 79: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/79.jpg)
Slip Field in the Specimen
Sl i p Fi el d i n the Speci men
0
1
2
3
4
5
6
7
8
0 1 2 3 4 5 6 7 8
Di stance to Top Surface (cm)
Slip
(*0
.1 m
m)
Speci men 10 Speci men 15 Li near Sl i p Fi el d Assumpti on
![Page 80: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/80.jpg)
Slip Field in the Specimen
The linear degree of slip field is 0.925. The assumption of linear slip field in RCED model is rational.
The size of the specimen influences the slip field lightly.
![Page 81: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/81.jpg)
Bond Stress along Steel BarStress Di stri buti on (10)
0
1
2
3
4
5
6
7
8
9
10
0 1 2 3 4 5 6 7 8
Di stence to Top (cm)
Sh
ear
Str
ess
(M
Pa)
Li near Assumpti on Resul t FEA Non-Li near Resul t
![Page 82: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/82.jpg)
Bond Stress along Steel Bar
Stress Di stri buti on(15)
0
1
2
3
4
5
6
7
8
9
10
0 1 2 3 4 5 6 7 8
Di stence to Top (cm)
Sh
ear
Str
ess
(M
Pa)
Li near Assumpti on Resul t FEA Non-Li near Resul t
![Page 83: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/83.jpg)
Change of Bond Stress
Bondi ng Stress Di stri buti on (Group 10)
0
1
2
3
4
5
6
7
8
9
10
0 1 2 3 4 5 6 7 8
Di stance to Top (cm)
Sh
ear
Str
ess
(M
Pa)
l oad1l oad2l oad3l oad4
![Page 84: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/84.jpg)
Conclusions
Obtain the full curves of the relationship of -1+2 . The empirical formula of -1+2 is obtained for the curves. Numerical study proves that this formula can be used in FEA directly.
The influence of specimen size to the local damage zone is not obvious.
The linear slip field in RCED model is rational
![Page 85: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/85.jpg)
Appendix
To apply the RCED model in real structure analysis.
Case 1: Using RCED model to analyze our test.
Case 2: Using RCED model to analyze the Doerr’s uniaxial-tension test (ASCE Vol.113, No.10, October, 1987)
![Page 86: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/86.jpg)
Mesh of Case 1
Common Concrete Element
RCED Element
![Page 87: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/87.jpg)
Result (-1+2 )
Δ 1+Δ 2
-2
0
2
4
6
8
10
12
-2 0 2 4 6 8 10
Δ 1+Δ 2(mm)
MPa
10s110s210s310s410s510s6fi tprogram
![Page 88: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/88.jpg)
Result (Deformation of Concrete)
-2
0
2
4
6
8
10
-0. 05 0 0. 05 0. 1 0. 15 0. 2 0. 25 0. 3 0. 35 0. 4
test poi nt 0. 1 0. 2 0. 4 0. 6 0. 85 0. 9 0. 95 1 12系列 3系列
![Page 89: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/89.jpg)
Mesh of Case 2
4 RCED elements250
150
![Page 90: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/90.jpg)
Result (Steel bar axial-force)
0
10
20
30
40
50
60
70
80
0 1 2 3 4 5 6 7 8
Forc
e (
KN
)
F=20KN, Test F=40KN, Test F=70KN, Test F=20KN, RCED F=40KN, RCED F=70KN, RCED
![Page 91: Experimental Study on the Damage Evolution of Re-bar Concrete Interface Lu Xinzheng SCE, THU CSE, NTU 1999/2000](https://reader035.vdocuments.site/reader035/viewer/2022062409/56649d265503460f949fd600/html5/thumbnails/91.jpg)
Element Number to Obtain the Same PrecisionTraditional element
Case 1
Element used: 656
Case 2
Element used: 192
RCED model
Case 1
Element used: 5
Case 2
Element used: 4
Conclusion: the element number RCED model
needed is much less than the traditional ones.
RCED model is useful in real structure analysis