![Page 1: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/1.jpg)
PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED HEAT EXCHANGERPrepared By: Mohammed Omer AbuALRub
Asset Engineering Dept.
SABIC Affiliate - Saudi Arabian Fertilizer Co (SAFCO)
April 2017
![Page 2: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/2.jpg)
No. 1
CONTENTS
Introduction
Brief Process Description
Schematic diagram of the cooling Water Circuit
Process Gas Cooler
Pitting Corrosion Phenomena
Heat Exchanger Inspection Strategy
Inspection Observation of Pitting Corrosion
Actions taken
Conclusion Remark
![Page 3: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/3.jpg)
No. 2
INTRODUCTION
In the process industry and petrochemical plants heat exchange coolers are essential and
important assets used to cool the process media by using cooling water as cooling media .
Cooling water to the process heat exchane coolers is supplied from closed loop cooling
water circuit in the plant. Usually, in cooling water circuits several heat exchangers are
present as per process requirements where heat exchange is achieved between process
media and cooling water. Heat exchange is exhibited at the heat transfer surface area of the
heat exchanger bundle tubes. In the bundle tubes, process media will be flowing at one side
and cooling water will be flowing at the other mating side of the tube. Process media will be
cooled due to cooling temperature effect of the circulated cooling water and heat of the
process media will be picked up by the flowing cooling water.
![Page 4: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/4.jpg)
No. 3
BRIEF PROCESS DESCRIPTION
The closed loop cooling water system supply cooling water to all heat exchange coolers in
the plant for cooling process media as per process requirement. The system consists of
centrifugal pumps, sea water cooled plate heat exchangers, cooling water tank and
connected piping system. Normally the turbine driven cooling water pumps remains on line
and motor driven pump remains on auto standby.
Both cooling water pumps takes water from cooling water storage tank and deliver it to
different plant users through the plate exchangers, where the returned hot cooling water is
cooled by exchanging heat with the sea cooling water. The cooling water system is closed
loop with corrosion inhibitor. Cooling water circulation supply pressure is (3.0 - 4.0) Kg/Cm2
and temperature is in the range of (30 - 40) °C.
![Page 5: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/5.jpg)
No. 4
00
SCHEMATIC FLOW DIAGRAM OF CLOSED LOOP COOLING WATER CIRCUIT
M
T
Cooling Water
Cooler
Process Gas
CW Pumps
CW
Distrib
ution
Header
Process Gas Cooler
Process
gas Inlet
Process
gas Outlet
00 0
Cooling Water Tank
Sea Water
PHE
Coolers
PHE: Plate Heat Exchanger
Sea Water
Sea
Water
Supply
Sea
Water
Return
![Page 6: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/6.jpg)
No. 5
PROCESS GAS COOLER
Shell Side Tube Side
Process Media Cooling Water Process Gas
Operating Pressure (Kg/Cm2) (3.0 – 4.0) (14.0 – 16.0)
Operating Temperature ( °C) (38 – 48) (161 – 46)
Material of Construction CS CS
Tube size - 19 mm dia
Years in service 1987
![Page 7: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/7.jpg)
No. 6
MAIN COMPONENTS OF THE PROCESS GAS COOLER
1) Shell component
2) Channel head component
3) Heat exchanger tube
4) Tube sheet
5) Baffle plates
6) Pass partition plate for U-Tube bundle
type
1
23
45
6
![Page 8: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/8.jpg)
No. 7
INTEGRITY OPERATING WINDOW (IOW) OF THE ASSET
Integrity Operating Windows (IOWs) are sets of defined limits used to determine the
different variables that could affect integrity and reliability of the asset.
It is important to develop limits for every possible damage mechanism that is likely to
affect the asset. This way, working within the limits set for the asset will be able to
prevent most likely types of damages that could affect the asset integrity.
In our case, operating pressure, temperature, process gas composition, cooling water
chemistry (i.e: pH, conductivity, TSS (Total Suspended Solids), corrosion inhibitor) are
important factors of the operating window.
![Page 9: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/9.jpg)
No. 8
ZONE OF THE INTEGRITY OPERATING WINDOW (IOW)
High Level
Low Level
Target High
Target Low
Target Optimum
High Critical Level
Low Critical Level
O
P
E
R
A
T
E
Z
O
N
EThe middle zone area
between (High – Low) is
the designated zone for
long term optimum
operate zone of the asset
![Page 10: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/10.jpg)
No. 9
PITTING CORROSION
Adherence of suspended solids from the electrolyte at the protection passive film of the
parent metal will cause localized damages to the passivation layer and initiation of localized
corrosion pit. Underneath, localized pitting corrosion attack can be a particularly severe form
of corrosion because of the difficulty in detection due to the corrosion occurring beneath the
material. Examples of these materials could be sand particles, dirt, corrosion products
“rust”, and other solid particles in the electrolyte system. Settlement of the material acts as
shield and creates stagnant condition underneath similar to the crevice corrosion type
attack.
Solids in suspension of the electrolyte solution tends to settle on the heating surface of the
heat exchanger tube. Pitting corrosion is one of the destructive corrosion type as it can lead
to equipment failure due to localized perforation with only small amount of iron weight loss.
![Page 11: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/11.jpg)
No. 10
ILLUSTRATION OF PITTING CORROSION ATTACK
e- e- e-
Process Gas
e-e-e-e-e-
e-e-
e-
OH-
OH-
OH-OH-
![Page 12: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/12.jpg)
No. 11
Localized corrosion pit
Passive Film Layer
Heat Exchanger Tube
![Page 13: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/13.jpg)
No. 12
PITTING CORROSION IMPORTANT REMARKS
Pitting is a form of localized corrosion attack at the metal surface.
The corrosion pits could be shallow in nature or large in diameter.
Corrosion pits some times are isolated or close to each other and form together rough
surface appearance.
Pitting corrosion is difficult to detect because of small size and mostly covered with
corrosion products
It is difficult to measure quantitatively by NDT (Non Destructive Testing) technique due to
small volumetric loss
Pits usually grow in the direction of gravity
The mechanism of pit growth is similar to that of crevice corrosion.
Velocity effect, pitting is usually associated with low flow velocity areas.
Increasing velocity of the circulating media often decreases pitting corrosion attack.
![Page 14: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/14.jpg)
No. 13
Inspection Strategy
RBI Study
Analysis
Generate inspection task with frequency
Visual Inspectio
n
UT Thickness check
NDT Tube Inspectio
n
NDT of TTS weld
joints
RBI Re-Assessment after inspectio
n
HEAT EXCHANGER INSPECTION STRATEGY
RBI (Risk Based
Inspection) approach
is used to develop
inspection strategy of
the asset
![Page 15: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/15.jpg)
No. 14
OBSERVATIONS DURING THE PLANNED INSPECTION
Tube bundle was pulled out from the shell and localized pitting corrosion attack found on
the tube external surface.
Baffle plates found free from pitting corrosion
Channel head and shell internal surface found free from pitting corrosion
Tubes internal surface found free from corrosion attack
Tube to tube sheet weld joints found free from defects
Tubes were inspected by MFL NDT technique.
![Page 16: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/16.jpg)
No. 15
PITTING CORROSION OF CS TUBE
Slightly deep corrosion pits
Shallow corrosion pits Baffle plate w/o signs
of corrosion pits
![Page 17: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/17.jpg)
No. 16
SHELL INTERNAL SURFACE
Internal surface of the shell
w/o signs of corrosion pits
![Page 18: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/18.jpg)
No. 17
ACTIONS TAKEN
1) Tubes with deep corrosion pits were plugged from both sides of the tube.
2) Tubes with shallow corrosion pits were left and kept under monitoring.
3) Shell side hydro test to ensure integrity of the tube bundle.
![Page 19: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/19.jpg)
No. 18
CONCLUSION REMARKS
1) In spite of localized corrosion pits, the tube bundle of the cooler had demonstrated
good service life under the operating window of the asset.
2) Operating the asset within the integrity operating window is very important and
essential for reliable operation of the asset and achieve optimum service life.
3) Keeping the solid particles in suspension state can minimize the sedimentation effect
at the heat transfer surface of the heat exchanger tube and consequence potential
effect of localized pitting corrosion attack
4) Monitoring and maintaining water chemistry including the corrosion inhibitor within the
specified limit is essential for the protection passivation layer and corrosion protection
of the asset.
4) Periodic timely inspection of the asset, is important for health condition assessment of
the asset.
5) Areas prone for relatively low circulation flow velocity in the circuit, shall have close
attention and inspection focus.
6) Side stream filtration system can be considered and evaluated as filtration option to
clean and remove solid particles from the electrolyte.
![Page 20: PITTING CORROSION OF CS HEAT EXCHANGER TUBE …nace-jubail.org/Meetings/JCMEF 2017/PD1/3. Abul-Rub-Presentation... · PITTING CORROSION OF CS HEAT EXCHANGER TUBE OF PROCESS GAS COOLED](https://reader031.vdocuments.site/reader031/viewer/2022013104/5b3246e27f8b9aa0238c12c9/html5/thumbnails/20.jpg)
No. 19