Download - molding defect(TH)
-
7/25/2019 molding defect(TH)
1/14
91 69 22 - 2552
(Injection Molding)
[13, 14] (Mold design) (Material properties)
Defects of Injection Molded Parts:
Causes and Troubleshooting
1
(Injection temperature) (Injection speed) (Holdingpressure) (Moldtemperature) [5, 6]
:
1
-
7/25/2019 molding defect(TH)
2/14
92 .
-
(Short shots)
1(a)
(Shot size)
1. (Injection temperature)2.
(Mold temperature)
3. (Injection pressure)
4. (Injection speed)
5. (Back pressure)
6. (Non-return valve)
1. / (Runner)2.
(Gate)3.
(Wall thickness)
4. (Venting)
1(a) (b) [5]
(a) (b)
-
7/25/2019 molding defect(TH)
3/14
93 69 22 - 2552
(Sink marks)
(Holding pressure) (Injection phase) (Shrinkage)
(Rib) 1(b)
1.
(Cushion)
2. /
3. -/ / (
)
4. -// ( )
5. (Cooling time)
6.
1.
2.
/
1. (Additives)
Chemical blowing agents (CBA) [11] (
CO2 N2) (Voids) (Core layer)
2. ( CO
2 N
2) (Gas/Water
assisted injection molding) [9, 13]
(Part sticking)
2(a)
-
7/25/2019 molding defect(TH)
4/14
94 .
1. /
/2. -//
3. 4.
(Mold release agents)
1.
(Ejector pins) (Symmetry)
2. (Cavity)
3.
(Multi-cavities)
4. (Stationary plate) (Sprue)
(Sprue puller) (Sprue bushing)
(a) (b)
2(a) (b) [3]
-
7/25/2019 molding defect(TH)
5/14
95 69 22 - 2552
(Flash)
2(b) (Parting line) (Ejectormarks)
1. (Clamping force)2. /
3. -/
4. /-
1.
2. (Venting)
3.
(Weld lines)
1 /
3(a) [12]
3(a) (b)
[7]
(a) (b)
-
7/25/2019 molding defect(TH)
6/14
96 .
(
) [5, 6, 4] 3(b)
1. -/
2. /
3. (Back pressure)
1.
2.
3.
1. Sequential valve gates
[8]
2. Push-pull injectionmolding [12]3. SCORIM (Shear control
orientation injection molding) [10]
(Jetting)
4(a)
//
1. -
2.
-
7/25/2019 molding defect(TH)
7/14
97 69 22 - 2552
(Blister)
(
) 4(b)
1. //
2. (Barrel)
Back pressure /
4(a) (b) [3, 4]
Suck back (
Drooling [16]) // Feedzone /
(a) (b)
-
7/25/2019 molding defect(TH)
8/14
98 .
(Voids/Bubbles)
5 (Blisters)
(Shrinkage) (Core layer) (Sol id if ied
skin layer/Frozen layer) ( ) (Vacuum)
5 [3]
1. (Cushion) /
/
2. -//
3. Back pressure (Meltdensity)
4.
1.
2.
3.
-
7/25/2019 molding defect(TH)
9/14
99 69 22 - 2552
4.
(Silver streaks)
(Moister)
6(a)
1.
2.
3.
4. Suckback
6(a) (b) [3]
(a) (b)
(Burn marks)
8001,000 oC
6(b)
-
7/25/2019 molding defect(TH)
10/14
100 .
1.
2.
/
3. Suckback
1.
2.
(Conta-
mination)
7(a)
(Pigments)
(Purging)
(Burn marks)
1.
(Hopper)
2. (Purging)
3. (Regrind) (Virgin) (Crusher)
4.
/// Polyvinyl Chloride (PVC)
5.
-
7/25/2019 molding defect(TH)
11/14
101 69 22 - 2552
(Blush marks)
7(b)
1.
2. /
Cold slug3.
(Shrinkage)
- (0.1-2.5%) (Semi-crystalline)
(Amorphous)
(Pressure) (Volume) (Temperature) PVT diagram [2]
1.
//
2. -//
3.
/
7 (a) (b) [3]
(a)(b)
-
7/25/2019 molding defect(TH)
12/14
102 .
(Warpage/Distortion)
8(b)
1.
2. //
3. -/ /
8(a) (b)
(a) (b)
1.
(Cooling path)
2.
8(b)3.
4.
-
7/25/2019 molding defect(TH)
13/14
103 69 22 - 2552
Data Handbook, Van NostrandReinhold, New York, 1989.
[7] Faculty of Mechanical and PlasticsEngineering, Chemnitz Universityof Technology, Germany.
[8] I. Khnert, V. Stoll and G. Mennig,The 21st annual meeting of thepolymer processing society (PPS),Leipzig, Germany, 19-23 June2005, ISBN 3-86010-784-4.
[9] J. Avery, Gas-Assisted InjectionMolding: Principle and Applicat-ions, Hanser Publishers, New York,2001.
[10] L. Wang, P.S. Alan and M.J. Bevis,Plastic Rubber and CompositesProcessing and Applications, 1995,
23(3): 139-150.[11] R.A. Malloy, Plastic Part Designfor Injection Molding, HanserPublishers, New York, 1994.
[12] S. Patcharaphun and G. Mennig,Journal of Reinforced Plastics andComposites, 2006, 25(4): 421-435.
[13] T.A. Osswald, Polymer ProcessingFundamentals, Carl Hanser Verlag,Munich 1998.
[14] T.L. Richardson and E. Lokensgard,Industrial Plastics: Theory andApplications, Delmar PublishersInc., New York, 1996.
[1] ARBURG GmbH, A Brief Guideinto Injection Molding, PostfachLossburg, Germany, 1999.
[2] A.W. Birley, B. Haworth andJ. Batchelor, Physics of Plastics:P r oce s s i n g , P r op e r t i e s an d
Materials Engineering, HanserPublishers, New York, 1992.
[3] Bakelite AG / KISTLER, Defects onInjection Molded Parts.
[4] D.M. Bryce, Thermoplastic Trouble-shooting for Injection Molders,Society of Plastic Engineers, 1991.
[5] Donald V. Rosato and DominickV. Rosato, Inject ion MoldingHandbook: The Complete MoldingOperation Technology, Perfor-mance, Economics, Chapman &Hall, New York, 1995.
[6] D.V. Rosato, Plastics Processing
-
7/25/2019 molding defect(TH)
14/14
104
[15] W. Michaeli, A. Brunswick and C.Kujat, Kunststoffe Plast Europe,2000, 90(8): 25-28.
[16] W. Michael i et al . , Trainingin Inject ion Molding, HanserPublishers, Munich 1995.