![Page 1: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/1.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
1
Casting Defects and Design Issues
ver. 2
![Page 2: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/2.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
2
Overview
• Processes
• Analysis
• Defects
• Design rules
• Economics
![Page 3: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/3.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
3
Issues in Casting
• Shrinkage
• Porosity
• Piping
• Microstructure
![Page 4: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/4.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
4
Shrinkage
• Can amount to 5-10% by volume
• Gray cast iron expands upon solidification due to phase changes
• Need to design part and mold to take this amount into consideration
![Page 5: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/5.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
5
Shrinkage
TABLE 5.1
Metal or alloy
Volumetric
solidification
contraction (%) Metal or alloy
Volumetric
solidification
contraction (%)
Aluminum 6.6 70%Cu–30%Zn 4.5
Al–4.5%Cu 6.3 90%Cu–10%Al 4
Al–12%Si 3.8 Gray iron Expansion to 2.5
Carbon steel 2.5–3 Magnesium 4.2
1% carbon steel 4 White iron 4–5.5
Copper 4.9 Zinc 6.5
Source: After R. A. Flinn.
![Page 6: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/6.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
6
Casting Defects
![Page 7: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/7.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
7
Defects - Hot Tears
![Page 8: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/8.jpg)
Steam Engine Flywheels
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
8
![Page 9: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/9.jpg)
Car Rims
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
9
Stamped Cast
![Page 10: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/10.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
10
Casting Defects - Porosity
![Page 11: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/11.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
11
Porosity
• Types
– due to gases – smooth bubbles
– due to shrinkage – rough voids
• Not a problem for ingots
– parts that will be deformation processed
– as long as it is not exposed to air (corrosion)
– can be healed
![Page 12: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/12.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
12
Porosity due to Gases
• Smooth bubbles
– result from entrapped gases
– solubility in liquid is high, in solid is low, so gas is rejected during cooling
• Sievert’s law
S = kpg0.5
– S = solubility
– k = constant
– pg = partial pressure of gas over melt
![Page 13: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/13.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
13
Remedies for Gas Bubbles
• Control atmosphere
– vacuum
– gases with less solubility
• Proper venting to let gases out
• Proper design of runners and gates to avoid turbulence
![Page 14: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/14.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
14
Remedies for Gas Bubbles
• Add metallic elements to react with gases
– killed steels - highly deoxidized (Al, Si)
• high shrinkage due to gas removal - piping
– semi-killed steels - less deoxidized
• less piping, porosity
– rimmed steels - little deoxidization
• blow holes in ring at rim (sometimes break through)
• little piping because gas doesn’t escape
![Page 15: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/15.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
15
Porosity due to Shrinkage
• Rough bubbles - voids
• Stages
– cooling liquid
– rejects latent heat at melting point
• alloys become slushy - liquid and solid co-exist
– cooling solid
![Page 16: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/16.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
16
Differential Cooling
• Transition between thicker and thinner sections can lead to porosity
![Page 17: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/17.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
17
Porosity / Shrinkage Solutions
• Risers allow molten metal to flow into mold to make up for shrinkage
• Design flow so no part freezes early
– large channels
• “Flexible” molds
– allow metal to shrink, not hold metal
![Page 18: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/18.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
18
Porosity / Shrinkage Solutions
• Heating or cooling certain areas to maintain uniform cooling (thermit or chills)
• Uniform part thickness
– leads to uniform cooling, less residual stress
![Page 19: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/19.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
19
Chills
![Page 20: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/20.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
20
Pipe Defect
• Due to shrinkage giving rise to a funnel-like cavity
• Solutions
– insulate top (glass wool)
– heat top (exothermic mixture - thermit)
![Page 21: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/21.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
21
Microstructure
![Page 22: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/22.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
22
Grains on Willie B’s head
![Page 23: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/23.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
23
Microstructure - Dendrites
• Finer structure at walls
• Grains / dendrites grow to center
![Page 24: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/24.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
24
Microstructure - Dendrites
![Page 25: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/25.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
25
Microstructure
• Post-treatment may be necessary to get desired properties - grain structure
– annealing
– tempering
– cold working
![Page 26: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/26.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
26
Design Rules Summary
• Uniform wall thickness
• Flat parting lines
• Gradual thickness transitions
• Draft for removal
– tapers: 0.5 to 2 degrees
• Surface of mold gives surface of part
![Page 27: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/27.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
27
Sand Casting Rules
![Page 28: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/28.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
28
Economics Example - Optical Bench
![Page 29: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/29.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
29
Requirements
• Casting of Al-Si alloy
• Number
– one-off
– preliminary run (100)
– production run (10,000)
• High precision required
– machining required
– pick cheapest casting method
![Page 30: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/30.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
30
Alternative Processes
• Sand casting
• Low pressure casting
• Permanent mold casting
• Die casting
![Page 31: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/31.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
31
Cost Equation
n
C
n
CCC
Lc
m&
++=
• C = cost/part
• Cm = material cost
• Cc = capital cost
• CL = labor cost
• n = number produced
• = production rate n&
![Page 32: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/32.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
32
Process Costs
Process SandCasting
LowPressure
PermanentMold
Die Casting
Material, Cm ($) 1 1 1 1
Labor, CL ($/hr) 20 20 20 20
Capital, CC ($) 0.9 4.4 700 3000
Rate, (#/hr) 6.25 22 10 50n&
![Page 33: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/33.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
33
Process Economics
![Page 34: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/34.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
34
Process Selection
• Probably pick low pressure casting, as a preliminary run of 100 is assured.
• If production run is needed, die casting will probably be used.
• The tough part is getting the process cost data.
![Page 35: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/35.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
35
Production of Aluminum Auto Parts MainCharacteristic
CastingGravity
ALow-PressureDie Casting
BHigh-PressureDie Casting(Pores Free)
C
SqueezeCasting
D
Pouring/FillingMethod
Ladle Air pressurethrough stalk
High-speed andhigh-pressureinjection byhydraulic piston
Relatively low-speed andhigh-pressureinjection
Filling Time (s) 10-30 10-30 1 10OperatingPressure (atm.)
1 1+(0.2-0.5) 100-500 500-1,000
Cycle Time(min.)
5-10 5-10 1-2 2
Die/MoldTemperature
High High Low Low-medium
DimensionalAccuracy
+ ++ +++ +++
DesignAvailability
+++ ++ + +
Productivity + ++ +++ +++Quality + ++ +-+++ +++Cost + + +++ +++MachiningRequired
Many Many Few Few
Main Parts(other thanwheels)
Intake manifold,cylinder blockand head,piston
Cylinder block,cylinder head,suspension,member
Cylinder block,oil pan, cylinderhead cover,transaxle case
Piston, disk-brake caliper,power steeringtoe control hub,knuckle
![Page 36: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/36.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
36
Advantages of Casting
• Near- or net- shape
• Less scrap
• Intricate shapes
• Large hollow shapes
• No limit to size
![Page 37: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/37.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
37
Disadvantages of Casting
• Shrinkage, porosity, cracks
• No strain hardening
– can be brittle
• Tooling can be expensive
– part shape depends on tool (mold)
• Microstructure can be difficult to control
– non-uniform cooling
– faster on outside produces finer grain structure there
![Page 38: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/38.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
38
Summary
• Defects
• Design rules
• Economics
![Page 39: Casting Defects and Design Issues · Die Casting B High-Pressure Die Casting (Pores Free) C Squeeze Casting D Pouring/Filling Method Ladle Air pressure through stalk High-speed and](https://reader031.vdocuments.site/reader031/viewer/2022013107/5cfdddbd88c99323308bee87/html5/thumbnails/39.jpg)
ME 6222: Manufacturing Processes and Systems Prof. J.S. Colton © GIT 2011
39