Atomic Layer Deposition: From Development to Commercialization
Steven M. George Depts. of Chemistry & Mechanical Engineering
University of Colorado, Boulder, Colorado 80309
![Page 2: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/2.jpg)
Examine Some Case Studies
Where has ALD been successfully commercialized?
What were the critical developments?
What were the critical needs?
How did ALD meet the unmet needs?
2
![Page 3: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/3.jpg)
Case Studies
1. Electroluminescent & Insulating Layers for Flat Panel Displays
2. High k Gate Dielectrics for MOSFETs 3. Isolation in Magnetic Read Heads
4. Low Leakage, High k Capacitors for DRAM
3
![Page 4: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/4.jpg)
Thin Film Electroluminescent (EL) Flat Panel Displays
Figure from T. Suntola, ALD2004 in Helsinki
4
Structure of Thin Film EL Display Energy Band Diagram
![Page 5: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/5.jpg)
Needs for EL Flat Panel Display Device
→ Technology in 1970s could not respond to these needs.
→ ALD could meet these needs. 5
1. Pin-Hole Free, Insulating & Barrier Films 2. High Quality, Thin Luminescent Films 3. Ability to Deposit on Large-Area Substrates
![Page 6: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/6.jpg)
Development of ZnS ALE
Elemental Precursors Molecular Precursors
Figure from T. Suntola, Ann. Rev. Mater. Sci. 15, 177 (1985). 6
First performed by Tuomo Suntola in August/September 1974 as reported by Suntola at ALD2004.
![Page 7: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/7.jpg)
Development of ALE Equipment
Equipment described in T. Suntola & J. Antson, U.S. Patent #4,058,430 (1977).
Equipment for ZnS growth in August/September 1974.
Figure from T. Suntola, ALD2004 in Helsinki 7
![Page 8: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/8.jpg)
Early Commercialization
Photo from T. Suntola, ALD2004 in Helsinki
First ALD Public Display: EL Display in Helsinki Airport, 1983-1998
Finlux, part of Lohja, starts making EL flat panel displays
in 1977. T. Suntola leads development project.
8
![Page 9: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/9.jpg)
Thin Film EL Display Production
Present Day Thin Film EL Displays from Lumineq (formerly Planar EL Displays). Lumineq is division of Beneq.
TFEL display manufacturing started in late 1970s and was only application of ALD for ~20 years.
9
![Page 10: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/10.jpg)
Outline
1. Electroluminescent & Insulating Layers for Flat Panel Displays
2. High k Gate Dielectrics for MOSFETs 3. Isolation in Magnetic Read Heads
4. Low Leakage, High k Capacitors for DRAM
10
![Page 11: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/11.jpg)
Gate Dielectric in MOSFET
Metal oxide semiconductor field effect transistor (MOSFET) is main switch used in silicon microprocessors.
11
![Page 12: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/12.jpg)
Need for High k Gate Dielectric
Miniaturization led to reduction of SiO2 gate dielectric thickness.
At SiO2 gate oxide thickness ≤ 10 Å, tunneling caused high current leakage.
High k materials were needed to achieve same capacitance with no tunneling.
→ Ultrathin and conformal films of new materials on silicon substrates.
12
![Page 13: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/13.jpg)
Cover of Semiconductor International, October 2001
Need for ALD for high k gate dielectrics leads to introduction of ALD on
International Technology Roadmap for
Semiconductors (ITRS).
![Page 14: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/14.jpg)
Development of HfO2 ALD
Figure from J.P. Chang in High-k Gate Dielectric Deposition Techniques, High Dielectric Constant Materials (Springer-Verlag, New York, 2005).
Chemistry developed by M. Ritala, M. Leskela et al., Thin Solid Films 250, 72 (1994).
14
![Page 15: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/15.jpg)
Nucleation Difficulties During HfO2 ALD on Si(100)
M.L. Green et al., J. Appl. Phys. 92, 7168 (2002). 15
![Page 16: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/16.jpg)
HfO2 Islands Observed after HfO2 ALD on H-Si(100)
E.P. Gusev et al., Microelect. Eng. 69, 145 (2003).
Islands
16
![Page 17: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/17.jpg)
Crystallization Temperature Depends on Al2O3 Mole% in HfO2
A.R. Londergan et al., ECS Proceedings, Vol. 2002-11, page 163. 17
![Page 18: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/18.jpg)
Development of ALD Equipment
18
ASM Pulsar 3000
Cross Flow Reactor Design
Figures from Suvi Haukka, ASM Microchemistry, “Role of ALD in Development of Ever-Shrinking Semiconductor Devices”, FinNano,
September 15-16, 2009.
![Page 19: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/19.jpg)
High k gate dielectrics introduced by Intel in 2007 for 45 nm CMOS technology.
Initial Commercialization by Intel
K. Mistry et al., Electron Devices Meeting, 2007. IEDM 2007. IEEE International, p. 247-250.
Hafnium-based high k gate dielectric with SiO2
equivalent oxide thickness (EOT) of 1.0 nm.
19
![Page 20: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/20.jpg)
Samsung 32 nm High k Metal Gate PMOS Transistor
Reverse Engineering by Chipworks
Hf-based high k gate dielectric
Gate oxide thickness ~2.0 nm
TiN metal gate
From Dick James at Chipworks, “Leading Edge Si Devices: an Update”
20
![Page 21: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/21.jpg)
Outline
1. Electroluminescent & Insulating Layers for Flat Panel Displays
2. High k Gate Dielectrics for MOSFETs 3. Isolation in Magnetic Read Heads
4. Low Leakage, High k Capacitors for DRAM
21
![Page 22: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/22.jpg)
Demanding Needs for Magnetic Isolation in Read Heads
Requirements for Dielectrics: Gap Isolation Using Al2O3:
Breakdown strength > 5 MV/cm Al2O3 by PVD Leakage currents < 10 µA/cm2 at 1V > 50 nm, RF Sputtering Thermal conductivity >1.0 W/mK < 50 nm, Reactive Sputtering Al2O3 PVD fails at < 20 nm
Figures and information from M. Kautzky, ALD2003 in San Jose 22
![Page 23: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/23.jpg)
Linear Growth Rate of Al2O3 ALD on NiFe Magnetic Substrate
Figure from M. Kautzky, Intermag (2008)
ALD able to provide controlled Al2O3 thicknesses
at < 20 nm
23
![Page 24: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/24.jpg)
Current-Voltage Curves for Various Al2O3 ALD Film Thicknesses on n-Si(100)
1 E-11
1 E-09
1 E-07
1 E-05
1 E-03
1 E-01
0 1 2 3 4 5 6 7 8 9 10Applied Potential (V)
Cur
rent
Den
sity
(A/c
m2 )
30 Å
60 Å 184 Å122 Å
1152 Å597 Å360 Å
Al2O3 ALD Provides Excellent Dielectric Films
Low Leakage. Similar to Thermal SiO2 Films
M.D. Groner et al., Thin Solid Films 413, 186 (2002).
24
![Page 25: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/25.jpg)
Performance of Al2O3 ALD Led to Rapid Development at Seagate
Device Yield from Al2O3 ALD Greatly Exceeded Al2O3 from Sputtering
September-October 2000: Tool and Film Evaluations
January 2001: Purchase Order for First Tool April-July 2001: Delivery/ Install/ Qualification of
First Tool
Information from M. Kautzky, Private Communication 25
![Page 26: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/26.jpg)
ALD in Spin-Valve Read Heads
AlTiC substrate
Basecoat
Bottom Shield
Top Shield
Bottom Pole
Top Shield
Bottom Shield Read Sensor
Gap2
Perm. Magnet
Contact
Gap1
Figures and information from M. Kautzky, ALD2003 in San Jose
Spin-valve sensor based on “current in plane”
Spin-valve heads in production for 5-6 years
Al2O3 ALD thickness ~20 nm 26
View of Air Bearing Surface
![Page 27: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/27.jpg)
Permanent Magnetic Isolation in Tunneling Magnetic Resistance (TMR)
Read Heads
Top shield
PM PM
Al2O3 Insulator Al2O3 InsulatorSeedAFMSAF
BarrierFL
Cap
Bottom shield
Top shield
Bottom shield
PMPM
Top shield
PM PM
Al2O3 Insulator Al2O3 InsulatorSeedAFMSAF
BarrierFL
Cap
Bottom shield
Top shield
Bottom shield
PMPM
Top shield
PM PM
Al2O3 Insulator Al2O3 InsulatorSeedAFMSAF
BarrierFL
Cap
SeedAFMSAF
BarrierFL
Cap
Bottom shield
Top shield
Bottom shield
PMPM
Read heads change from spin-valve to TMR in ~2005
Figure from M. Kautzky, Intermag (2008) 27
![Page 28: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/28.jpg)
TMR Read with ALD Permanent Magnet Isolation
M. Kautzky et al., IEEE J. Magnetics 44, 3576 (2008).
TMR sensor based on “current perpendicular
to plane” TMR sensor for read
width of ~20 nm Al2O3 ALD thickness
of ~5 nm
28
![Page 29: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/29.jpg)
Outline
1. Electroluminescent & Insulating Layers for Flat Panel Displays
2. High k Gate Dielectrics for MOSFETs 3. Isolation in Magnetic Read Heads
4. Low Leakage, High k Capacitors for DRAM
29
![Page 30: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/30.jpg)
Requirements for Metal-Insulator-Metal (MIM) Capacitors for DRAM
DRAM requires high k dielectric because of miniaturization
Low leakage needed for stable
charge storage
Conformality critical because of high aspect ratio structures
30
![Page 31: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/31.jpg)
ALD Provides Conformality in Trench Capacitor Structures
Trench with aspect ratio of ~60 & minimum lateral dimension of
~80 nm
~100% conformality for 18 nm thick Al2O3
ALD film
From “Atomic Layer Deposition for Advanced DRAM Applications”, Future Fab Intl. Issue 14 (2/11/2003), by
M. Gutsche et al. from Infineon Technologies AG 31
![Page 32: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/32.jpg)
ALD of HfO2/Al2O3 Nanolaminates Yields Low Leakage, High k Insulators
Al2O3 20 Å Al2O3:HfO2 15%:85% 50 Å Al2O3:HfO2 80%:20% 30 Å Al2O3:HfO2 20%:80% 40 Å Al2O3:HfO2 65%:35% 20 Å Al2O3:HfO2 35%:65% 30 Å Al2O3 20 Å
Figures from O. Sneh et al., Thin Solid Films 402, 248 (2002). 32
![Page 33: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/33.jpg)
ITRS DRAM Roadmap
Table from International Technology Roadmap for Semiconductors, 2009 Edition 33
![Page 34: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/34.jpg)
DRAM MIMCap Based on TiN/ZAZ/TiN Structure
Demonstrated in 2006 by Hynix Semiconductor
ZAZ is tri-layer of ZrO2/Al2O3/ZrO2
TiN, ZrO2 and Al2O3 by ALD
J.A. Kittl et al., Microelect. Eng. 86, 1789 (2009). 34
![Page 35: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/35.jpg)
STEM Analysis & Performance of ZAZ Stack
Dielectric stack is ~10 nm
SiO2 EOT of 0.85 nm
Low leakage of ~10-8 A/cm2 at 1V
J.A. Kittl et al., Microelect. Eng. 86, 1789 (2009). 35
ZrO2
![Page 36: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/36.jpg)
ALD Semiconductor Equipment Market
Results from VLSI Research, Inc.
36
![Page 37: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/37.jpg)
Review of Case Studies
1. Electroluminescent & Insulating Layers for Flat Panel Displays
2. High k Gate Dielectrics for MOSFETs 3. Isolation in Magnetic Read Heads
4. Low Leakage, High k Capacitors for DRAM
37
![Page 38: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/38.jpg)
Conclusions from Case Studies
For Successful ALD Applications: ALD has been able to respond to a critical need
when no other method could meet the need.
Future is Promising: ALD is still moving into fields that are just beginning to appreciate the benefits of ALD.
38
![Page 39: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/39.jpg)
Additional Developments on Horizon
1. ALD for Passivation of Silicon Wafers 2. ALD on Polymers as Gas Permeation Barriers
3. ALD for Energy Applications 4. ALD for Materials Enhancement
39
![Page 40: Atomic Layer Deposition: From Development to Commercialization George... · 2015-02-27 · Atomic Layer Deposition: From Development to Commercialization. Steven M. George Depts](https://reader033.vdocuments.site/reader033/viewer/2022043019/5f3b5167b8891366d04a8fa7/html5/thumbnails/40.jpg)
Acknowledgements
ALD in MOSFET and DRAM: Tom Seidel (formerly Aixtron/Genus) Michael Current (Current Scientific)
Risto Puhahka (VLSI)
ALD in Magnetic Read Heads: Mike Kautzky (Seagate)
Other Contributions: Erwin Kessels (Eindhoven)
Greg Parsons (NC State)
40